JASC 5310
Service difficulty reports · 38,573
Reports filed under 5310 · Fuselage Main, Structure, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5310' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5310' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR IPXA09M57780Torque Box · cracked3/8 INCH CRACK IN CORNER OF CUTOUT IN UPPER TORQUE BOX FOUND DURING TAIL TANK TRANSFER PIPE INSPECTION EO MD11-2820-14180-K MAJOR REPAIR - REPAIRED PER EO MD11-5310-35352-ASDR USAA2009102692873Door Frame · corrodedPIT - FPBH - MAJOR REPAIR - CORROSION ON FUSELAGE AFT DOOR FRAME AT BS 847, S27R. REPLACED FUSELAGE AFT DOOR FRAME AT BS 847, S27R.SDR ZZDA2009318Door Frame · corrodedAFT CARGO DOOR JAMB, STA 954 TO 994, CORROSION. ACCOMPLISHED CARGO DOOR JAMB PAN SPLICE REPAIR PER B717 SRM 53-20-15 REPAIR 7 FIG 201. SEE NR 3695 AND 2687.SDR ASOA200901174Post · crackedFOUND FS 409+128 IB SIDE VERTICAL POST RBL 18.0 HAS AN INDICATION NOTED APPROX .2" IN LENGTH 50% FSH AT WL 49.0 AFT FLANGE RADIUS. FAILED NDT INSPECTION. REMOVED VERT POST ASSY AT FS 409+128 RBL 18 IAW SRM 51-42-06 AND 51-42-21. REQUIRES NEW I/B POST. INSTSDR COEA2009102209821Crease Beam · damagedHEAVY CHECK COE: MAJOR REPAIR, CARGO COMPARTMENT CREASE BEAM RIGHT SIDE FWD OF FRAME 24 UNDERSIDE OF WEB HAS SEVERAL TOOLING MARKS. REMOVED RT CREASE BEAM WEB BETWEEN FR23D AND FR24. BLENDED TOOLING MARKS IAW ATR72 DO\TS SRI 12468. RE-INSTALLED CREASE BEAMSDR FDEA200910213641Torque Box · crackedAFT AIRSTAIRS, RT LR TORQUE BOX, LWR LIGHTNING HOLE IS CRACKED AT BS 1223. REMOVED DAMAGE 1/4" X 3/4" IN AFT AIRSTAIR RT LWER TORQUE BOX LOWER LIGHTNING HOLE AT BS 1213 IAW SRM REV 101 51-10-1. FABRICATED DOUBLER IAW SRM 51-40-2 FIG 1 AND 53-10-2 FIG 6. INSTASDR FDEA200910213640Torque Box · crackedAFT AIRSTAIRS, RT LWR TORQUE BOX, LWR LIGHTNING HOLE IS CRACKED AT BOTTOM AT BS 1213. REMOVED DAMAGE 1/4" X 3/4" IN AFT AIRSTAIRS RT LOWER TORQUE BOX LOWER LIGHTNING HOLE AT BOTTOM BS 1213 IAW B727 SRM REV 101 51-10-1. FABRICATED DOUBLER FROM 7075T6 .032SDR FDEA200910213639Torque Box · crackedAFT AIR STAIRS, RT LWR TORQUE BOX, LWR LIGHTNING HOLE IS CRACKED AT TOP AT BS 1213. REMOVED DAMAGE 1/4" X 3/4" IN AFT AIRSTAIRS RT LOWER TORQUE BOX LOWER LIGHTNING HOLE AT BS 1213 IAW B727 SRM REV 101 51-10-1. FABRICATED DOULBER FROM 7075T6 .032" X 4" X 2 SDR FDEA200910213643Door Frame · looseR2 DOOR UPPER HINGE OPENING HAS LOOSE FASTENERS AT OLD REPAIR. R2 UPPER HINGE OPENING REPAIRED IAW EA F-5210-133427 (R2 DOOR CRACK REPAIR). REPAIR IS CLASSIFIED AS MAJOR IAW GMM 6-2-100.SDR FDEA200910213642Door Frame · crackedL2 DOOR UPPER HINGE OPENING HAS CRACK. CRACKED L2 DOOR UPPER HINGE OPENING REPAIRED IAW EA F-5210-133417 (L2 DOOR CRACK REPAIR). REPAIR IS CLASSIFIED AS MAJOR IAW GMM 6-2-100.SDR FDEA200910203619Crease Beam · corrodedSTA 1277- 1287 LT CREASE BEAM CORRODED. REMOVED CREASE BEAM IAW SRM 51-40-02, FABRICATED NEW BEAM FROM MAT BAC1515-5537075T6511, IAW SRM 51-30-01, INSTALLED CREASE BEAM STA 1180-1290, LBL 60, IAW SRM 51-40-02, MAJOR REPAIR.SDR ZZDA2009322Door Frame · corrodedAFT CARGO DOOR JAMB, STA 954 TO 994, CORROSION. ACCOMPLISHED CARGO DOOR JAMB PAN SPLICE REPAIR PER B717 SRM 53-20-15 REPAIR 7 FIG 201. SEE NR 3343 AND 3430.SDR ZZDA2009317Door Frame · corrodedFWD CARGO DOOR JAMB, STA 372 TO 425, CORROSION. ACCOMPLISHED CARGO DOOR JAMB PAN SPLICE REPAIR PER B717 SRM 53-20-15 REPAIR 6 FIG 201. SEE NR 3694 AND 3767.SDR FDEA200910193611Frame · dentedCABIN - RT STA 1641, L-11 TO L-12 FRAME FOUND DENT. REPAIRED IAW SRM 53-00-07 FIG 201, REV 41. INITIAL INSP TO BE CARRIED OUT AT 14,500 FLT CYCLES AND SUBSEQUENT REPETITIVE INSPECTIONS AT EVERY 9,500 FLIGHT CYCLES IAW SRM 53-00-07, TABLE 201. REPAIR 2, REV SDR FDEA200910193609Frame · dentedCABIN - RT STA 1761, L-11 TO L-12 FOUND DENT. REPAIRED IAW SRM 53-00-07 FIG 201. REPAIR 2, REV 41. INITIAL INSP TO BE CARRIED OUT AT 14,500 FLIGHT CYCLES AND SUBSEQUENT REPETITIVE INSPECTIONS AT EVERY 9,500 FLIGHT CYCLES IAW SRM 53-00-07, TABLE 201, REPASDR FDEA200910193608Frame · chafedCABIN - LT STA 1781, L-11 TO L-12 FOUND CHAFED. REPAIRED IAW SRM 53-00-07 FIG.201. REPAIR 2 REV 41 INITIAL INSP TO BE CARRIED OUT AT 14,500 FLIGHT CYCLES AND SUBSEQUENT REPETITIVE INSP AT EVERY 9,500 FLIGHT CYCLES IAW SRM 53-00-07, TABLE 201. REPAIR 2, REV SDR FDEA200910193607Frame · dentedCABIN - LT STA 1761, L-11 TO L-12 FOUND DENT. REPAIRED IAW SRM 53-00-07 FIG 201. REPAIR 2 REV 41 INITIAL INSP TO BE CARRIED OUT AT 14,500 FLIGHT CYCLES AND SUBSEQUENT REPETITIVE INSPECTIONS AT EVERY 9,500 FLIGHT CYCLES IAW SRM 53-00-07, TABLE 201, REPAIR 2 SDR FDEA200910183604Torque Box · crackedAFT AIRSTAIR AREA - RT LWR TORQUE BOX, LWR LIGHTNING HOLE IS CRACKED BS 1223. CUT OUT DAMAGED AREA IAW SRM 51-10-1 REV 101, FABRICATED DOUBLER IAW SRM 53-10-2 FIG 6 AND 51-40-2 FIG 1. INSTALLED REPAIR DOUBLER ON RT LOWER TORQUE BOX IAW SRM 51-30-2 REV 101.SDR SIMA200929301Structure · corrodedDURING MAINTENANCE INSPECTION, FOUND THE LAVATORY BUCKET HAS CORROSION. AIRCRAFT REMOVED FROM SERVICE. FABRICATED AND INSTALLED DOUBLER IAW SRM 53-31-02. AIRCRAFT RETURNED TO SERVICE.SDR ASOA200901193Structure · corrodedMAIN AVIONICS COMPARTMENT FS 333, STR 26L - STR 27 CTR HAS CORROSION COMMON TO FRAME.SDR ASOA200901162Support Beam · crackedACM/ ECU SUPPORT BEAM CRACKED AT OTBD END AT FS 718 STR 11.SDR FDEA200910163594Crease Beam · corrodedMAIN CABIN STA 660-680 LT SIDE INBD CREASE BEAM CORD HAS CORROSION (OUT OF LIMITS). REMOVED CORROSION BS 66-680, LBL 63, FOUND OUT OF LIMITS IAW SRM 53-30-15, FIG. 101, 45 PERCENT THROUGH MATL. REMOVED CREASE BEAM, BS 565-755, LBL 63. FABRICATED NEW CREASE BSDR FDEA200910163592Crease Beam · corrodedLT CREASE BEAM CORRODED BS 1320-1360. REMOVED CORROSION IAW SRM 53-60-15 ORIG MAT .100, MAT LOSS .012 FOUND TO BE OUT OF LIMITS IAW SRM 53-60-15 FIG.101 DET 3, REMOVED AND REPLACED CREASE BEAM STA 1290-1370, LBL 58 IAW SRM 51-40-02, MAJOR A REPAIR.SDR FDEA200910163591Crease Beam · damagedMAIN CABIN BS 1634, RBL 60 CREASE BEAM FASTENER HOLE ELONGATED. REPAIR CARRIED OUT ON BEAM IAW STA, EA 757-5361-08-E0439 REV.- (ELONGATED HOLE FOUND ON 146N8722-43 CHORD, STA 1620 TO 1640 RT). REPAIR IS CLASSIFIED AS MAJOR IAW GMM 6-2-100 CRITERIA.SDR ZZDA2009311Door Frame · corrodedAFT CARGO DOOR JAMB CUTOUT AREA HAS CORROSION STA FROM 954 TO 994. INSTALLED AFT CARGO COMPARTMENT DOOR JAMB LOWER SPLICE REPAIR PER B717 SRM 53-20-15 REPAIR 7 FIGURE 201. SEE NR 3797, 3829 AND 2382.SDR QXEA2009101600807Buttstrap · corrodedEVIDENCE OF CORROSION FOUND ON BUTT STRAP AT 280 BETWEEN STR 24L AND 25L. REMOVED FASTENERS FOR ACCESS IAW 51-42-6. REMOVED CORROSION IAW SRM 51-21-06-001-001-A01 FOUND TO BE WITHIN LIMITS IAW REO 670-53-11-450. PERFORMED LPI ON STR 24L AND 25L NO CORROSIOSDR QXEA2009101600806Fitting · corrodedEVIDENCE OF CORROSION FOUND ON INTERNAL FWD JACK FITTING ON LT JACK FITTING SUPPORT SKIN ATTACH FLANGE AND WEB JUST FWD OF FS 280. REMOVED FASTENERS FOR ACCESS IAW 51-42--6-001-001-A01. REMOVED CORROSION IAW SRM 51-21-06-001-001-A01 FOUND TO BE OUT OF LIMITSSDR QXEA2009101600805Fitting · corrodedEVIDENCE OF CORROSION FOUND ON INTERNAL FORWARD JACK FITTING ON RT JACK FITTING SUPPORT SKIN ATTACH FLANGE JUST FWD OF FS 280. REMOVED CORROSION IAW SRM 51-21-06-001-001-A01 FOUND TO BE WITHIN LIMITS PER REO 670-53-11-450. PERFORMED EDDY CURRENT INSPECTION .SDR QXEA2009101600803Buttstrap · corrodedEVIDENCE OF CORROSION ON BUTT STRAP A FS 280 BETWEEN STR 25R AND 26R. BLENDED AREA AND FOUND TO BE OUT OF LIMITS. RECEIVED REO 670-53-11-450. PERFORMED LPI ON BLEND NO CORROSION FOUND AT THIS TIME IAW NDTM 51-20-006. TREATED, PRIMED, PAINTED AND APPLIED CORSDR FDEA200910153581Crease Beam · corrodedRT CREASE BEAM UPPER SURFACE CORRODED, BS 1440-1460. (OUT OF LIMITS) REMOVED CORROSION FROM RT CREASE BEAM, BS 1405-1680, IAW SRM 51-40-02. EXFOLIATION CORROSION FOUND TO BE OUT OF LIMITS IAW SRM 53-60-13, FIG 101, .060" MATERIAL LOSS. FABRICATED NEW CRSDR FDEA200910153578Vertical Beam · misinstalledFASTENERS HAVE NO SPACING AFT PIT BS 1183 LBL 17.8 VERTICAL BEAM. TRIMMED OUT BS 1183 BULKHEAD WEB APPROX DIM: 30 1/2" X 9 1/4", BULKHEAD BEAM CUT-OUT DIM: 33 5/8". FABRICATED BULKHEAD WEB REPAIR DOUBLERS, FILLER. FABRICATED BEAM REPAIR TEE REPAIR ANGLES, FSDR DL757100201Failsafe · corrodedFUSELAGE FAIL SAFE STRAP CORRODED, RT SIDE AT STA 900 CP53-232-01I / REPLACED FAIL SAFE STRAP AT SAT SAA REF NON ROUTINE CARD 141457.SDR QXEA2009101600796Structure · corrodedDURING INSP FOUND CORROSION PRESENT AT FS 813 STR 27 BETWEEN APPROX RBL 4" TO LBL 4". REMOVED RIVETS FOR ACCESS IAW SRM 51-42-00-001-001-A01. BLENDED OUT CORROSION FOUND WITHIN LIMITS, TREATED, PRIMED, INSTALLED RIVETS AND PAINTED IAW SRM 51-21-06, 53-31-06,SDR SIMA200928902Rib · crackedDURING MAINTENANCE INSPECTION, FOUND A CRACK ON THE RIGHT AFT BULKHEAD AROUND THE RIGHT MAIN LANDING GEAR. CRACK LENGTHS WERE 6/8 OF AN INCH AND 1 INCH. AIRCRAFT REMOVED FROM SERVICE. REPAIRED CRACKS ON RIGHT BULKHEAD AFT SECTION IAW EMB SRM 53-23-12. AIRCSDR FDEA200910143574Door Frame · crackedMAIN CABIN FOUND CRACK ON WEB JAMB DOOR. REPAIRED AREA IAW SRM 53-50-00 FIG 19 VOL I.SDR FDEA200910133551Crease Beam · corrodedLT CREASE BEAM CORRODED AT UPPER AND LWR SURFACE, BS 1540-BS1620 (OUT OF LIMITS). REMOVED CORROSION IAW SRM 51-10-02. ORIG MATERIAL THICKNESS; .070", AFTER REWORK; .059". FOUND TO BE OUT OF LIMITS IAW SRM 53-60-13, FIG 101. REMOVED LH CREASE BEAM, BS 1370-1SDR FDEA200910133550Crease Beam · corrodedMAIN CABIN, STA 480, RT SIDE CREASE BEAM CHORD HAS CORROSION (OUT OF LIMITS). REMOVED CORROSION AND CHECKED LIMITS IAW SRM 51-10-02/53-30-13. FOUND TO BE OUT OF LIMITS IAW SRM 53-30-13, FIG.101,DETAIL 3 AT BS 450-665, RBL 60. ORIGINAL MATERIAL THICKNESS- .070SDR ASAA0976786Crease Beam · corrodedCORROSION AT A FASTENER ON LT CREASE BEAM WEB UPPER SURFACE. REMOVED CREASE BEAM WEB, FABRICATED NEW WEB AND INSTALLED.SDR C2XA09SH335Door Frame · corrodedSHV - DURING C-CHECK MAIN DOOR AFT CUTOUT (FRM 18) HAS CORROSION (LEVEL 2 LOCAL) AROUND SCREW HOLES BETWEEN STR 14L-15L. MAINTENANCE PERFORMED REPAIR ON MAIN DOOR AFT CUTOUT (FRM 18)BETWEEN STR'S 14L-15L IAW EMB-145XR EC5310-01482. THE AIRCRAFT WAS APPROVED SDR ZZDA2009308Door Frame · corrodedAFT CARGO DOOR JAMB CUTOUT AREA HAS CORROSION STA FROM 954 TO 994. INSTALLED AFT CARGO COMPARTMENT DOOR JAMB LOWER SPLICE REPAIR PER B717 SRM 53-20-15 REPAIR 7 FIGURE 201. SEE NR 3797, 3829 AND 2382.SDR AALA20091009TUL03Stop Fitting · crackedFORWARD CARGO DOOR STOP PAD FITTING AT FORWARD END OF NUMBER 2 BEAM CRACKED. REMOVED STOP PAD FITTING NUMBER 2 AND INSTALLED NEW FITTING PER ESO80174.SDR FDEA200910093533Vertical Beam · misinstalledFUSELAGE STA 1183 LWR CHORD LT INBD 17.8 VERT BEAM FASTENERS SPACING SHORT. REPAIR ACCOMPLISHED ON NON-ROUTINE N00323 UNDER WORK ORDER 00045711 IAW EA 7-5310-126851.SDR ZZDA2009307Door Frame · corrodedFWD CARGO DOOR JAMB AREA HAS CORROSION FROM STA 370-427. CUT OUT DAMAGED LOWER SECTION AND INSTALLED NEW LOWER SECTION AND SPLICES, REPAIR PER REF B717 SRM 53-20-15 REPAIR 6.SDR AALA20091019TUL08Door Frame · crackedCRACK EXTENDING FROM FASTENER HOLE IN RIGHT NOSE LANDING GEAR DOOR JAMB BEAM AT STATION 48. REPAIRED CRACK PER AARD 53-10-00-4.SDR FDEA200910083500Crease Beam · misalignedDURING INSTALLATION OF INNER CREASE BEAM CHORD AT STA 640, 2 EA EXISTING HOLES WERE FOUND THAT CANNOT BE PICKED UP. COMPLIED WITH EA 757-5331-16-F2284 AT STA 640, LBL 58, ON MAE WORK CARD 118350403BZ2R01. THIS NON ROUTINE IS FOR TRACKING PURPOSES ONLY. (MAJOSDR C2XA09TY255Skin · crackedLEFT WINDSHIELD POST SKIN CRACKED. CUT AND REMOVED AREA OF CRACKED SKIN. FABRICATED AND INSTALLED FILLER AND DOUBLER IAW EC5310-01483.SDR ZZDA2009270Door Frame · damagedINSTALLED FWD CARGO LOWER JAMB PAN SECTION AND SPLICE REPAIR PER B717 SRM 53-20-15 FIGURE 201. SEE NR 3040 AND 3244.SDR FDEA200910083516Vertical Beam · damagedAFT CARGO COMPT, BS 1183 PRESSURE BULKHEAD LBL 17.8 VERTICAL BEAM WEB HAS SEVERAL DOUBLE DRILLED HOLES AT WL 190. REPAIR ACCOMPLISHED ON NON-ROUTINE N00323 UNDER WORK ORDER 00045711 IAW EA 7-5310-126851, REFERENCE SDR 09-3493.SDR FDEA200910083511Crease Beam · corrodedLBL 62 FLOORBOARD SUPPORT FS, 395-377 CORRODED REMOVED CORROSION IAW SRM 51-10-02. ORIGINAL MAT .050 MAT LOSS IS .050 FOUND TO BE OUT OF LIMITS IAW SRM 53-0051 FIG 101 DETAIL 2 RMOVED CREASE BEAM IAW SRM 51-40-02. FABED NEW ON TRAVELER NR T9/ 804601 IAW SRMSDR SWAA096409Door Frame · crackedDURING SCHEDULED 20Y CHECK, FOUND R1 DOOR UPPER STUB FRAME CRACKED. REMOVED AND REPLACED FRAME SECTION PER BAC DWG.
Back to JASC 5310