JASC 5310
Service difficulty reports · 38,573
Reports filed under 5310 · Fuselage Main, Structure, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5310' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5310' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR 05FDEA00735Shear Web · corrodedCORROSION IN SHEAR WEB BS 1166 LBL 29-33 WL 208.SDR 05FDEA00749Door Frame · corrodedAREA BEHIND BULK CARGO BETWEEN FRAMES 72-74 LEFT SIDE AT STRINGER 49 HAS 15 SQ" OF CORROSION. REMOVED CORROSION FR 72-74 FOUND TO BE OUT OF LIMITS IAW A310-200 SRM 53-10-00 FIG 104. REMOVED AND REPLACED STRINGER SECTION 49L FR 72 TO 78 IAW A310-200 SRM 53-SDR 05FDEA00744Beam · corrodedMAIN DECK CARGO CLS ADAPTER BETWEEN R1 AND R2 AT FRAME 50 IS CORRODED. REMOVED AND REPLACED BEAM IAW A310-200 SRM 51-72-10.SDR UIEA200500043Beam · crackedD-CHECK, DURING SCHEDULED INSPECTION, CRACKS WERE FOUND AT THE NOSE GEAR WELL ON THE VERTICAL BEAM WEBS AT LHS BS 280L, 300L, 320L AND 320R. DAMAGED PORTION OF THE VERTICAL BEAM WEB WAS TRIMMED OUT AND A NEW SECTION OF THE WEB WAS SPLICED IN. NOTE: THESE RSDR SWAA050952Post · crackedDURING SCHEDULED 1/4D CHECK, FOUND R1 COCKPIT WINDOW POST CRACKED AT UPPER OUTBOARD CORNER. REPAIRED WINDOW POST PER SRM.SDR DHL2005740539Torque Box · crackedREF. FLIGHTSTAR NR 104834 DISCREPANCY - RT LOWER TORQUE BOX CRACKED AT ST 1230. CORRECTIVE ACTION - STAP DRILLED CRACK .250 TERMINATED AT END OF CRACK ON RH LOWER TORQUE BOX BS1230 IAW B727 SRM 51-10-1. HFEC INSP. PER 727 NDT PT.6 51-00-00 FIG.23 NO CRACKS NOTSDR DHL2005740536Torque Box · crackedRT LOWER TORQUE BOX CRACKED AT STA 1223. STOP DRILLED CRACK .250 TERMINATED AT END OF CRACK ON RT LOWER TORQUE BOX STA 1223 IAW B727 SRM 51-10-1, HFEC INSP PER NDT PT.6 51-00-00 FIG 23. CRACK ENDS IN STOP HOLE. FABRICATED DOUBLER REPAIR IAW B727 SRM 53-10-2SDR SWAA050943Crease Beam · corrodedDURING SCHEDULED 1/2D CHECK, FOUND FUSELAGE CREASE BEAM WEB CORRODED AT BS 638, RBL 65. REPAIRED WEB PER SWA EA & SRM.SDR SWAA050942Crease Beam · crackedDURING SCHEDULED 1/2D CHECK, FOUND FUSELAGE CREASE BEAM WEB CRACKED AT BS 616, RBL 64. REPAIRED WEB PER SWA EA & SRM.SDR 05FDEA00668Structure · corrodedBETWEEN FRAME 91 AND 95 (AFT OF THS BOX) BILGE AREA AND AROUND ACCESS THRESHOLD 300 SQ INCHES OF BARE METAL WITH LITE SURFACE CORROISION. REMOVED AND REPLACED CORRODED STRUCTURE AT FR91 TO 95 AND STR 16 LT IAW A310 SRM 51-40-21 AND DWG'S A53989325, A53989300,SDR QXEA200500534Structure · damagedPDX - SHEET METAL PIECE JUST AFT OF LEFTHAND FORWARD NOSE LANDING GEAR DOOR ON NOSE LANDING GEAR SIDEWALL IS PUSHED UP AND CRUMPLED. REPAIRED IAW DHC-8-400 SRM 51-42-05.SDR MALA050297Structure · corrodedDURING 4K CHECK IN BNA FOUND LAV SERVICING PORT P/N 7253680-117 HAS BEEN REPLACED DUE TO HEAVY CORROSION IAW SRM 51-40-22.SDR SWAA050879Fitting · crackedDURING SCHEDULED C2 CHECK, FOUND L1 DOOR LOWER FUSELAGE HINGE BOX FITTING CRACKED. REMOVED AND REPLACED HINGE BOX FITTING PER SRM & SAM 326.SDR ABXA050082Door Frame · crackedDOOR JAMB WAS CRACKED AT TOP LEFT STOP AT INBOARD RIVET. REPAIRED DOOR JAMB AT TOP LEFT IAW DC-9 SRM 53-05.SDR DHL2005805676Heat Exchanger · crackedA 0.500 CRACK IN SKIN OF RT PRIMARY HEAT EXCHANGER AFT UPPER CORNER STA -12.000 L-24R (MAJOR REPAIR). PERFORMED MAJOR REPAIR IAW FAA FORM 8110-3 DATED 03-16-05 DWG X83-R07 REV IR DATED 03-16-05. REMOVED FASTENERS IAW SRM 51-1-21 PG 1. CUT OUT DAMAGED SECTIOSDR DHL2005805673Heat Exchanger · crackedA 0.250 CRACK IN LT PRIMARY HEAT EXCHANGER AFT LWR CORNER STA -12.000 L-27L (MAJOR REPAIR). PERFORMED MAJOR REPAIR IAW FAA FORM 8110-3 DATED 03-16-05 DRAWING X83-R04 REV IR DATED 03-01-05. REMOVED FASTENERS IAW SRM 51-1-21 PG 1. CUT OUT DAMAGED SECTION IAW SDR 05FDEA00616Shear Web · corrodedCORROSION ON SHEAR WEB WITH 100 PERCENT MATERIAL LOSS AT BS 1140-1145, LBL 57-62, WL 208. REPLACED SHEAR WEB PER SRM 51-40-2SDR 05FDEA00610Structure · corrodedDURING INSPECTION FOUND AT STA 1741 STRUCTURE X=-17; X= 17 WITH CORROSION AND RETAINER X= 17 WITH CORROSION. REMOVED CORROSION FROM AFFECTED AREA PER SRM 51-21-01. PERFORMED CHECK LIMITS; THE MATERIAL REMOVED IS WITHIN LIMITS PER SRM 53-00-01. PROTECTED ASDR DHL2005805530Frame · misdrilledMAIN CARGO COMPT FRAME INBD FLANGE HOLES (2EA) MISDRILLED AT STA 1420.000 L-12 AND L-13L. PERFORMED MAJOR REPAIR IAWW FAA FORM 8110-3 DATE 03-05-05, EO NR AST050205 DATE 02-21-05. CLEANED, TREATED AND PRIMED (AREA) MISDRILLED HOLES IAW SRM 51-1-8B. PERFORMESDR SWAA050854Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON CREASE BEAM WEB BETWEEN BS 480 & BS 500, STR 17L. REPAIRED CREASE BEAM PER SRM.SDR MALA050280Structure · corrodedDURING 4Y/2Y CHECK IN BNA FOUND CORROSION ON UPPER AND LOWER SURFACES AND BETWEEN SPLICES AT STA 258. REMOVED CORROSION, OUT OF LIMITS. FABRICATED AND INSTALLED REPAIR ANGLES REF SAAB SRM 53-10-30; 51-20-42; 51-40-21.SDR 2005UALA00249Tear Strap · corrodedTEAR STRAP AT STA 1400 BETWEEN STR 27L AND 28L IS CORRODED. DAMAGE CAUSED BY TYPICAL CORROSION. TEAR STRAP REPAIR AND EXTERNAL DOUBLER WAS INSTALLED.SDR SWAA050800Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON CREASE BEAM WEB AT BS 300, WL 208, RBL 50. REPAIRED WEB PER SRM.SDR 05FDEA00544Doubler · damagedREPAIR NEEDS EVALUATION FOR FAA APPROVED DATA AND MAJOR OR MINOR CLASSIFICATION ITEM NR 5 FUSELAGE, L-SHAPED DOUBLER RT SIDE ABOVE RT WING AT FR44 L-SHAPE DOUBLER, RT SIDE ABOVE WING AT FRAME A310-200 SRM 53-15-12 FIG 1 SHEET 9.SDR SWAA050771Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND L1 DOOR CREASE BEAM WEB CORRODED BETWEEN BS 312 TO BS 344, LBL 63, WL 208. REPAIRED CREASE BEAM PER SRM.SDR SWAA050783Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CREASE BEAM WEB CORRODED AT BS 370, STR 17L. REMOVED AND REPLACED WEB SECTION PER SRM.SDR SWAA050775Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CREASE BEAM CORRODED BETWEEN BS 867 TO BS 887, LBL 67, WL 208. REPAIRED CREASE BEAM PER SRM.SDR SWAA050774Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CREASE BEAM CORRODED BETWEEN BS 727C TO BS 727E, RBL 67, WL 208. REPAIRED BEAM PER SRM.SDR USAA050363Forging · crackedCLT - C5 - FORGING, .3 INCH, CRACKED, FWD SERVICE DOOR CUTOUT UPPER FWD UPPER CORNER. REMOVED CRACKED REVEL AND REPLACED IAW DWG NR 65-55878. (K)SDR 05FDEA00485Door Frame · chafedC/W EA8-5310-55459 FUSELAGE-MAIN FRAME-AFT ENTRY DOOR JAMB REPAIR (P/N AJC7207- 181). CLOSING ACTION 03/10/05 C/W EA8-5310-55459. ON NO. S00017.SDR SWAA050725Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON CREASE BEAM WEB AT BS 385, STR 17L. REMOVED AND REPLACED CREASE BEAM WEB SECTION PER SRM.SDR SWAA050724Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON CREASE BEAM WEB BETWEEN BS 747 TO BS 767, LBL 70, WL 208. REMOVED AND REPLACED CREASE BEAM WEB SECTION PER SRM.SDR COMA0570026Beam · corrodedFS 280 LT AND RT BULKHEADS AND TRANSVERSE BEAM HAVE MAJOR CORROSION ON AFT SIDE ALONG THE BOTTOM EDGES. REPLACED LOWER WEBS AT FS 280 BULKHEAD IAW BOMBARDIER, INC. REO 670-53-11-052, REV A REPAIR NR 2 AND BRAS E.O. 601R-53-6066. REPLACED TRANSVERSE BEAM I/A/SDR 05FDEA00457Crossbeam · corrodedMDCC ZONE 250, FS 54.2 BETWEEN LT SEAT TRACK 4 -5, LATERAL STUCTURE HAS CORROSION AT SCREW HOLES. REMOVED AND REPLACED CROSS BEAM IAW A310-200 SRM 51-72-10.SDR 05FDEA00448Structure · corrodedAFT PIT UNDER FLOOR FROM 12 INCH FWD OF FS 59 TO 3 INCHES FWD OF FS 59 STG44L HAS CORROSION. REMOVED CORROSION IAW A310-200 SRM 51-74-10. THE AREA WAS FOUND OUT OF LIMITS IAW A310-200 SRM 53-10-00. REPAIRED STRINGER IAW A310-200 SRM 53-10-14. TREATED, PRIMESDR SWAA050714Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON CREASE BEAM WEB AT BS 363, STR 17R. REPAIRED WEB PER SRM.SDR 2005F00039Door Frame · crackedLOWER DOOR FRAME CRACKING BY THE REAR HINGE.SDR 2005UALA00216Crease Beam · corrodedRIGHT CREASE BEAM WEB CORRODED BETWEEN BS 1380 AND 1400 RT SIDE. DAMAGE CAUSED BY CORROSION TYPICAL FOUND ON CREASE BEAMS. CREASE BEAM WEB REPLACEMENT WAS FABRICATED AND INSTALLED.SDR SWAA050709Shear Tie · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON SHEAR TIE AT BS 1006, BL 0, WL 180. REMOVED AND REPLACED SHEAR TIE PER SRM.SDR SWAA050706Crease Beam · corrodedDURING SCHEDULED D-CHECK, FOUND CORROSION ON FUSELAGE CREASE BEAM WEB AT BS 410, STR 17R. REMOVED AND REPLACED CREASE BEAM WEB SECTION PER SRM.SDR LR7A05014Beam · crackedDURING SCHEDULED C5 INSPECTION PER JOB CARD HC5313 FOUND CW REAR BEAM WEB CRACKED AT FS 597, WL 276, CWS 52L. REPAIRED IAW LAC MEA 382-57-05-025.SDR 05FDEA00389Structure · corrodedBULKPIT UNDER FLOOR 5 INCHES AFT OF FR 65 STG 51R HAS AN AREA 1 X 1 INCH OF CORROSION EXTENDING UNDER FASTENERS. REMOVED CORROSION IAW A310-200 SRM 51-74-10. AREA WAS OUT OF LIMITS IAW A310-200 SRM 53-10-00. REMOVED AND REPLACED DAMAGED AREA IAW A310-200 SRSDR ASOA05206Doubler · crackedDURING AN A-CHECK IN BTR, THE DOUBLER AT FS 640, LBL 45 WAS FOUND TO BE CRACKED BEYOND LIMITS. MAINTENANCE IS REMOVING AND REPLACING THE DOUBLER AT FS 640, LBL 45. (M)SDR DHL2005805536Doubler · damagedEXTERNAL FUSELAGE RT NR 6 ACCESS DOOR JAMB HAS INTERIM REPAIR ON INTERNAL DOUBLER (MAJOR REPAIR). PERFORMED MAJOR REPAIR IAW SRM 53-1-0 PAGE 1, SRM 53-3-3 FIG 1. REMOVED EXISTING REPAIR DOUBLER (EXT) AND INTERNAL DOUBLER WITH INTERIM REPAIR IAW SRM 51-1-21 PSDR USAA050341Stringer Clip · crackedCLT - Q6 - STRINGER CLIP, .5 INCH CRACK, STATION 500A, STRINGER 16R. REPLACED WITH FABRICATED CLIP IAW SRM. (K)SDR 2005UALA00211Shear Tie · corrodedAFT PIT STA 1620, RBL 2 SHEAR TIE HAS CORROSION. REPLACEMENT SHEAR TIE WAS FABRICATED AND INSTALLED.SDR ABXA050067Structure · crackedCRACK IN SUBFLOOR STA 160 RBL 6. REPAIRED AREA IAW DC-9 SRM 53-01.SDR SWAA050662Window Post · crackedDURING SCHEDULED 1/4D CHECK, FOUND CRACK ON L1 UPPER WINDOW POST. REPAIRED L1 WINDOW POST PER SRM.SDR CA050304003Door Frame · cracked(CAN) WHEN COMPLYING WITH MFG REPETIVE SEB 03-5, A 2 INCH CRACK WAS DISCOVERED IN THE AREA OF THE LT LOWER DOOR HINGE ATTACH POINT ON THE DOOR POST. INSTALLED SERVICE KIT SK172-154TO REPAIR THE CRACK. NO INDICATIONS OF CRACKS ON THE RT SIDE.SDR 05FDEA00330Drain · corrodedCOMPLY WITH EA 8-5310-55454, FUSELAGE MAIN FRAME BULK CARGO DOOR LWR JAMB SILL CORROSION REPAIR (P/N AFA3248). CLOSING ACTION ON 02/28/05. ON N/R S00015, COMPLIED WITH EA8-5310-55454.
Back to JASC 5310