JASC 5320
Service difficulty reports · 216,095
Reports filed under 5320 · Fuselage Miscellaneous Structure, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5320' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5320' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR SWAA2025061773518Intercostal · crackedCRACKED INTERCOSTAL AT FWD WET AREA BS390 RBL41 WL208. REMOVED AND REPLACED ANGLE AT FLOOR STRUCTURE RBL 41 WL 208 BETWEEN BS 380 TO BS 400 PER SRM 51-40-02 AND DWG 143A5400 REV -.SDR SWAA2025061773519Intercostal · crackedCRACKED INTERCOSTAL AT FWD WET AREA BS394 LBL13 WL208. REMOVED AND REPLACED THE CRACKED INTERCOSTAL UPPER ANGLE FROM BS-380 TO BS-400; LBL13; WL208 IAW SRM 51-40-02 AND DWG#143A5400 REV:-.SDR SWAA2025061673482Angle · crackedCRACK ON ANGLE FWD FACE LOCATED BS 500C AT LEVEL STR 26L AT FWD CARGO COMPARTMENT 2025-340144<[01] REPLACED ANGLE FWD FACE LOCATED BS 500C AT LEVEL STR 26L AT FWD CARGO COMPARTMENT I.A.W B737-700 SRM 51-10-02 SRM 51-40-05; SRM 51-20-01 AND DWG 143A7505 SHEET 1SDR SWAA2025061673480Gusset · crackedCRACK GUSSET LOCATED BS 500D AT LEVEL STR 19R AT FWD CARGO COMPARTMENT 2025-340139<[01] REPLACED GUSSET LOCATED BS 500D AT LEVEL STR 19R AT FWD CARGO COMPARTMENT IAW B737-700 SRM 51-10-02 ITEM 9 DWG: 143A7902 SHEET: 209 REV: -. SEE INDIVIDUAL SIGN OFF BELOW;[0SDR SWAA2025061673481Gusset · crackedCRACK GUSSET LOCATED BS 500D AT LEVEL STR 19L AT FWD CARGO COMPARTMENT 2025-340143<[01] REPLACED GUSSET AND FASTENERS LOCATED BS 500D AT LEVEL STR 19L AT FWD CARGO COMPARTMENT I.A.W B737-700 SRM 51-10-02 ITEM 9; SRM 51-40-02 AND DWG: 143A7902; SHEET: 209; REV:SDR SWAA2025061673721Support Angle · crackedCRACK ON SUPPORT ANGLE LOCATED AFT FACE BS 500D AT LEVEL STR 28L AT FWD CARGO COMPARTMENT 2025-340160<[01] REPLACED SUPPORT ANGLE AND FASTENERS LOCATED AFT FACE BS 500D AT LEVEL STR 28L AT FWD CARGO COMPARTMENT I.A.W. B737-700 SRM 51-40-02; SRM 51-10-02 ITEM 9SDR SWAA2025061673478Support Angle · crackedCRACK ON SUPPORT ANGLE LOCATED BS 695 RBL 24.75 AT PASSENGER CABIN 2025-340131<[01] REPLACED SUPPORT ANGLE LOCATED BS 695 RBL 24.75 AT PASSENGER CABIN I.A.W B737-700 SRM 51-40-02; SRM 51-10-02 ITEM 9 AND DWG: 273A9110 SHEET: 6 REV: A<BR>SEE INDIVIDUAL SIGN OF SDR AALA202506130948Fitting · crackedAIRCRAFT IN BASE MAINTENANCE: CRACK ON INTERCOSTAL (HOLE 3) FITTING LOCATED FR 20 RH SIDE AT LEVEL STR 22 AND AT LEVEL DOOR STOP FITTING 1. CRACK DEPTH =0.055 INCH. MAINTENANCE REPLACED INTERCOSTAL FITTING LOCATED FR 20 AT LEVEL STR 22R AND AT LEVEL DOOR STOPSDR R61A2025061100287Splice Plate · corrodedCF3 INTERNAL, CORROSION FOUND ON FLOOR SPLICE PLATE AT FR84 RBL30. MX REPLACED SPLICE PN 170-86055-001 IAW SRM 51-43-01SDR R61A2025061100286Doubler · corrodedFWD FUSELAGE FR19 LBL30 FOUND CORROSION ON FLOOR SUPPORT DOUBLER. MX REPLACED SUPPORT DOUBLER PN 170-07311-003 IAW SRM 51-41-02, 51-43-04SDR ASAA2025052158405Web · corrodedAFT CARGO DOOR ENTRY, ENTRY DOOR THRESHOLD HAS CORROSION 3" AND ACROSS DOOR OPENING. (MARKED IN RED). GROUNDED - YES. REMOVED CORROSION FROM AFT CARGO DOOR THRESHOLD WEB, ORIGINAL THICKNESS; .050 1 REMOVED; .019, REMAINING: .031 AND FOUND TO BE OUT OF LIMITS ISDR JJBA20250602089Bracket · corrodedCORROSION FOUND AROUND LOWER BRACKET ON VENTRAL FUEL TANK FACE CENTER. REMOVED AND REPLACED VENTRAL TANK. OPS AND LEAK CHECK SAT.SDR IPXA2025052900464Stiffener · crackedCRACK - AFT CGO FLOOR BEAM & WEB & STIFFENER CRACK AT STA 1760 (REPAIR) 1.REPAIR DAMAGE AREA I.A.W UPS EO-93889-REQ1 REV.2 2.JOB COMPLETEDSDR IPXA2025052900526Floorbeam · crackedCRACK - AFT CGO FLOOR BEAM & WEB & STIFFENER CRACK AT STA 1780 (REPAIR) 1.REPAIR DAMAGE AREA I.A.W. UPS EO-93891-REQ1 REV.1 2.JOB COMPLETED.SDR DALA2025052704077Channel · corroded(LOG 0978726) CORROSION ON LH ZEE CHANNEL SIDEPLATE AT FLOOR STRUCTURE BTW STA 727-847 AND LBL 21 AT AFT CARGO COMPARTMENT. ZEE CHANNEL SIDEPLATE (LH) BTW STA 727-847 LBL 21 AT AFT CARGO COMPARTMENT, WAS REPLACED PER B737-800 SRM 51-40-02-0G.SDR DALA2025052704076Angle · corroded(LOG 0978507) R2 SERVICE DOOR ENTRY ANGLE BS 951-992 HAS MULTIPLE AREAS OF CORROSION. REMOVED AND REPLACED NEW R-2 DOOR CHORD SILL IAW B 737 SRM 51-40-02.SDR DALA2025052704075Angle · corroded(LOG 0978485) L2 ENTRY THRESHOLD ANGLE HAS MULTIPLE AREAS OF CORROSION. REMOVED AND REPLACED L2 DOOR CHORD SILL 147A8540U7 IAW B 737 SRM 51-40-02.SDR DALA2025052704071Channel · corroded(LOG 0977252) CORROSION ON RH ZEE CHANNEL SIDEPLATE AT FLOOR STRUCTURE BTW STA 727-767 AND RBL 21 AT AFT CARGO COMPARTMENT. RH ZEE CHANNEL SIDEPLATE AT FLOOR STRUCTURE BTW STA 727-767 AND RBL 21 AT AFT CARGO COMPARTMENT WAS REPLACED PER B737-800 SRM 51-40-02-0SDR CALA2025052304924Panel · wornAFT CARGO COMPARTMENT L/H FR49 BETWEEN STRINGER 32L-34L HAS ELONGATED FASTENER HOLE AT SLOPE PANEL SUPPORT PROFILE. REMOVED AND REPLACED SLOPE PROFILE PNL IAW 51-42-11/001.SDR SWIA2025052200021Angle · crackedRH INTERCOSTAL CLIP, AFT OF REAR PRESSURE BULKHEAD AT STGR 14R CRACKED (FILED OPEN)THIS IS CURRENTLY A WORK IN PROGRESSSDR AALA202505224497Floor Support · corrodedAIRCRAFT IN BASE MAINTENANCE: CORROSION ON FORWARD CABIN FLOOR BEAM BETWEEN FR 12 AND FR 24 AT +Y765. REPLACED FLOOR BEAM PER SRM 51-72-11.SDR DALA2025052203945Web · corrodedSHIP 3162 UPPER FUSELGE, FWD ENTRY AREA RIGHT SIDE, FLOORS STRUCTURE WEB BETWEEN FR20 AND FR21 WITH CORROSION. CORRECTIVE ACTION: REPLACED FLOOR STRUCTURE WEB LOCATED AT UPPER FUSELAGE FWD ENTRY AREA RIGTH SIDE BETWEEN FR20 TO FR21 IAW A319 SRM 51-72-11-911- 0SDR DALA2025052203943Web · corrodedSHIP 3135 CORROSION WEB LOCATED FROM FR20 TO FR24 AND STR 23R AT FWD GALLEY AREA. CORRECTIVE ACTION: REPLACED WEB LOC BTW FR 20R TO FR 24R AND STR 23R AT FWD GALLEY AREA AS PER A319 SRM 51-42-11, A319 SRM 51-72-11. (0978225).SDR UIEA2025052100660Bracket · damagedMAIN PASSENGER CABIN FWD STORAGE CLOSET MEGAPHONE BRACKET DAMAGED.(<P>REMOVED AND REPLACED MEGAPHONE BRACKET AT MAIN DECK FWD STORAGE CLOSET IAW B767 SRM 51-40-02. NO FURTHER DEFECTS NOTED.</P>)SDR HNAA2025080500485Web · crackedF048899 CABIN CENTER FLOOR SUPPORT WEB BETWEEN FR58 AND FR59 IS CORRODED AND POSSIBLY CRACKED. INSTALLED NEW FABRICATED DOUBLER ON CABIN CENTER FLOOR SUPPORT WEB BETWEEN FR58 AND FR59 IAW ETD2025-145-922732, PIEDMONT EO1-53-25-0219SDR AALA202508011308Intercostal · crackedAIRCRAFT IN BASE MAINTENANCE: CRACK ON INTERCOSTAL FITTING LOC. AT FR20 RH AT LEVEL DOOR STOP FITTIN G 7 PAX CABIN UPPER FUSELAGE L= 0.100. MAINTENANCE REPLACED INTERCOSTAL FITTING #7 LOCATED ON FR 20 BTW STRG 10 AND STRG 11 RH SIDE AT FWD GALLEY AREA. I.A.W.SDR SWAA2025063073239Intercostal · crackedCRACK WEB - INTERCOSTAL FLOOR STRUCTURE LOCATED BS344 TO BS 360 LBL 12 FWD GALLEY AND LAV 2025-335415 <[01]. REPLACED NEW WEB INTERCOSTAL LOC. ON FLOOR STRUCTURE BS344 TO BS 360 LBL 12 FWD GALLEY IAW B737-700 SRM 51-40-02-0G-0 AND DWG 141A5400 SHEET 46 REV A; SDR SWAA2025062473284Scuff Plate · crackedAFT CARGO BAY AFT CORNER SCUFF PLATE IS CRACKED<[01] AFT CARGO BAY AFT CORNER SCUFF PLATE REPAIRED PER SRM 53-60-15-2R-1<BR>ALL WORK COMPLETE ON CUSTOMER CARD TTG8Q010PPJ1.;[02] VERIFIED ITEM 1;[03] VERIFIED STEP 5 COMPLETE.SDR SWAA2025062473279Baffle · crackedFORWARD CARGO BAY 2 EA BAFFLE CLIPS ARE CRACKED BS500B AND 500C RBL25 WL156 FWD SIDE OF FRAME<[01] EVALUATED; REMOVED AND REPLACED THE BAFFLE CLIPS (2EA) AT BS 500B AND 500C RBL 25 WL 156 FWD SIDE OF FRAME PER SRM 51-40-02-0G-0 AND DWG 143A7505 REV: -.;[02] VESDR SWAA2025062473286Strap · corrodedCORROSION AFT CARGO BAY FLOOR SPLICE STRAP AROUND NUT PLATE HOLE BS767+6 RBL11.5 WL156<[01] EVALUATED CORROSION ON SPLICE STRAP; FOUND TO BE OUT OF LIMITS RECEIVED NEW SPLICE STRAP AND PAINTED ALL PER SRM 51-10-02; AND MM 51-21-73-370-804SDR SWAA2025062473288Support · corrodedCORROSION AFT CARGO BAY R/H FLOOR TO SIDEWALL SUPPORT PLATE HAS MULTIPLE AREAS AROUND NUT PLATE HOLES BS727B TO BS767 RBL22 WL156<[01] CORROSION ON AFT CARGO BAY R/H FLOOR TO SIDEWALL SUPPORT PLATE FOUND TO BE OUT OF LIMITS. REMOVED; REPLACED AND INSTALLED NEWSDR SWAA2025062473281Shield · corrodedCORROSION AFT CARGO BAY SHIELD FWD OF CARGO DOOR AROUND MULTIPLE NUT PLATE HOLES BS767+3 TO BS794 RBL22 WL156<[01] CORROSION ON SHIELD FOUND TO BE OUT LIMITS. REMOVED; REPLACED AND INSTALLED NEW SHIELD BS 767 TO BS 794 RBL 22 WL 156 PER SRM 51-40-02-0G-0; AND SDR SWAA2025062473282Plate · corrodedCORROSION AFT CARGO BAY L/H FLOOR TO SIDEWALL SUPPORT PLATE MULTIPLE AREAS AROUND NUT PLATE HOLES BS727B TO BS767 LBL22 WL156<[01] CORROSION ON AFT CARGO BAY L/H FLOOR TO SIDEWALL SUPPORT PLATE FOUND TO BE OUT OF LIMITS. REMOVED; REPLACED AND INSTALLED NEW L/HSDR SWAA2025062473285Scuff Plate · crackedFORWARD CARGO BAY AFT CORNER SCUFF PLATE IS CRACKED. REPAIRED FWD CARGO BAY AFT CORNER SCUFF PLATE PER SRM 53-30-15-2R-1<BR>ALL WORK COMPLETE ON CUSTOMER CARD TTG8Q010PPKP.SDR SWAA2025062473290Splice Strap · corrodedCORROSION AFT CARGO BAY FLOOR SPLICE STRAP AROUND NUT PLATE HOLE BS887 RBL11.5 WL163<[01] CORROSION ON STRAP WAS FOUND TO BE OUT OF LIMITS. REMOVED; REPLACED AND INSTALLED NEW FLOOR STRAP BS887 WL163 PER SRM 51-40-02-0G-0. DWG 147A7500 REV: - AND 146A7500 REV:SDR SWAA2025062373268Splice Plate · corrodedACB FLOOR PLATE SPLICE CORRODED AT BS887 BETWEEN LBL6-RBL6<[01] REMOVED AND REPLACED ON ACB FLOOR PLATE SPLICE BS887 RBL21 TO LBL 10 IAW SRM 51-40-02 AND DWG 146A7500 ID:0052 REV:B;[02] CORRECTIVE ACTION COMPLETED.SDR SWAA2025062073267Splice · corrodedACB FLOOR PLATE SPLICE CORRODED AT BS767+5 BETWEEN LBL10-RBL10. RECEIVED NEW ACB FLOOR PLATE SPLICE BS 767+5 LBL21 TO RBL21 ITEM 146A9401-4 LOT#1507361-1. LOCATED AND DRILLED IAW SRM 51-40-05. PART WILL BE INSTALLED IN CUSTOMER CARD TTG8Q00ZVPGH.SDR SWAA2025061772760Angle · crackedANGLE CRACKED I/B OF LH DEFECTION RIB (MPN 115A2156-7). REMOVED ANGLE PER SRM 51-40-02. LOCATED AND DRILLED FASTENER HOLES IN NEW ANGLE PER SRM 51-40-05. INSTALLED REPLACEMENT ANGLE PER SRM 51-40-02.SDR SWAA2025061772761Angle · crackedANGLE ASSY CRACKED I/B OF LH DEFECTION RIB (MPN 115A2156-17). REMOVED ANGLE PER SRM 51-40-02. LOCATED AND DRILLED NEW FASTENER HOLES IN NEW ANGLE PER SRM 51-40-05. INSTALLED REPLACEMENT ANGLE PER SRM 51-40-02. INSPECTED PER SRM 51-40-02-0G-0-B00069 (GENESDR R61A2025061100290Door Sill · corrodedCF3 AFT PASSENGER DOOR CUTOUT FOUND LOWER SILL CORRODED BTWN FR85-87. MX REPLACED BEAM PN 170-65703-005 IAW SRM 51-43-01, 51-43-02.SDR QXEA2025060400236Doubler · corrodedFWD WET AREA FWD RH DOUBLER CORRODED. FWD RH WET AREA DOUBLER FOUND TO BE OUT OF LIMITS IAW SRM 53-10-10 REPLACED DOUBLER IAW SRM 51-40-08.SDR DALA2025052704034Scuff Plate · corrodedAFT PAX DOOR (L2) SILL SCUFF PLATE AREA HAS EXTERNAL SKIN CORROSION AT HOLES 3OL, 4OL, 5OL, 8OL, 10OL, 11OL, & 12OL. REMOVED CORROSION, EVALUATED DAMAGE ON AFT PAX DOOR SCUFF PLATE AREA, FOUND OUT OF LIMITS IAW A220 ASRP J51-21-06, J53-62-33. RESTORED FINISH ASDR DALA2025052704033Door Sill · corrodedSSI : 53-61-24-02 R2 PAX DOOR SILL . CORROSION AT FASTENER HOLE 1/16 INCH IN LENGTH , 1/18 INCH WIDE AT FR 75. REMOVED CORROSION, EVALUATED DAMAGE AREA OF R2 PAX DOOR SILL, FOUND OUT OF LIMITS IAW A220 ASRP J51-21-06, J53-61-24. RESTORE FINISH AND PERFORMED COSDR DALA2025052704023Web · crackedSHIP 9572 INITIAL INSPECTION:CRACK ON MEMBRANE STA Y =692 X=-44 AT RH PASSENGER CABIN (CPAX). CORRECTIVE ACTION: REPAIRED PER B717-200 SRM 53-00-55. (0976468)SDR AALA202505274183Web · crackedAIRCRAFT IN BASE MAINTENANCE: CRACK IN RIGHT HAND SILL WEB FROM BS 927 TO BS 947 AT RBL 54. REPLACED WEB PER AARD 51-00-05-01 AND EA 364592.SDR DALA2025052203967Fitting · corroded(LOG 0976989) CORROSION WAS FOUND ON FITTING BTW STA. 907 AND BTW S-24L TO S-25L ALSO CORROSION WAS FOUND ON SUPPORT STA 927 BTW S-24L TO S-25L. FITTING BTW STA. 907 AND BTW S-24L TO S-25L AND SUPPORT STA 927 BTW S-24L TO S-25L WERE REPLACED PER B737-800 SRM 5SDR DALA2025052203964Intercostal · corroded(LOG 0976456) AFTER REMOVED INTERCOSTAL ON STA 907 TO 927 BTW S-24L TO S-25L WAS FOUND EXFOLIATION ON PART. INTERCOSTAL ON STA 907 TO 927 BTW S-24L TO S-25L WAS REPLACED PER B737-800 SRM 51-40-02-0G.SDR CALA2025052104892Floor Support · corrodedCABIN FLOOR SUPPORT Y 512.5 AT FR 68-70 HAS CORROSION. CABIN FLOOR SUPPORT Y512.5 AT FR68-70 RMVD + RPLCD IAW A320 SRM 51- 72-11-911-001 + 51-42-11/001.SDR CALA2025052104891Support · crackedAFT CARGO COMPARTMENT L/H BETWEEN FR 54-58 STRINGER 31L HAS CRA CKED AT SLOPE PANEL SUPPORT PROFILE. R & R NEW PROFILE PNL ON AFT CARGO FR54 TO FR58 STR31L IAW A320 SRM 51-42-11.SDR CALA2025052104890Angle · crackedRT AIR CONDITIONER BAY TO VAPOR BARRIER AFT UPPER ANGLE CRACKED AROUND MOST IB ATTACH FASTENER. REF. AAR N/R:9967538 GENERATED BY :V919797 ESFR INFORMATION ENTERED. ESFR ENTERED BY STEVE AST U180628 C/W
Back to JASC 5320