JASC 5743
Service difficulty reports · 3,097
Reports filed under 5743 · Wing, Landing Gear Attach Fittings, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5743' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5743' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR 2001UALA00425Fitting · crackedTHE LEFT MLG SUPPORT BEAM OUTBOARD SUPPORT FITTING IS CRACKED. SUPPLEMENTAL DATA UPDATE INSTALLED DOUBLER AND BOLTS. MAJOR REPAIR ACCOMPLISHED.SDR 2001UALA00397Fitting · damagedLT WING MAIN LANDING GEAR BEAM FITTING CRACKED. INSTALLED DOUBLER AND BOLTS. MAJOR REPAIR ACCOMPLISHED.SDR 2001UALA00396Fitting · damagedRT WING UPPER CHORD AND MAIN LANDING GEAR FITTING CRACKED. INSTALLED DOUBLER AND BOLTS. MAJOR REPAIR ACCOMPLISHED.SDR SWAA010954Fitting · corrodedDURING SCHEDULED D-CHECK, FOUND LT MLG AFT STABILIZER BEAM FITTING CORRODED. REMOVED AND REPLACED BEAM FITTING PER MM.SDR MALA010376Bushing · corrodedFOUND DURING C-CHECK, LT MLG OB TRUNNION PIN BUSHING HAS MIGRATED. MAINTENANCE REMOVED MIGRATING TRUNION PIN BUSHING ON LT OB MLG AND CLEANED AREA. INSTALLED TRUNION PIN BUSHINGS PER CMM 32-10-06. REFER TO IPM-12 FOR ALL REPAIRS DONE TO LHOB MLG.SDR 2001UALA00336Attach Fitting · damagedEXCESSIVE MATERIAL REMOVED DURING BLEND OUT ON RT MAIN LANDING GEAR SUPPORT BEAM ATTACH FITTING. REPLACED THE RT MAIN LANDING GEAR SUPPORT BEAM ATTACH FITTING. MAJOR REPAIR ACCOMPLISHED.SDR DL73K010500Fitting · corrodedCORROSION WAS FOUND IN A FASTENER HOLE OF THE UPPER ROW COMMON TO THE REAR SPAR UPPER CAP OF THE MLG SUPPORT BEAM O/B AFT FITTING. ANOTHER FASTENER HOLE WAS MISDRILLED WHILE REPLACING THE AFT FITTING. THE FASTENER HOLES WERE OVERSIZED AND BUSHED PER ERA 3973SDR AT0100126Attach Fitting · chafedFOUND RIGHT ATTACH FITTING FOR MLG CHAFED AT BS 737. BLENDED CHAFED AREA, TREATED, PRIMED AND INSTALLED IAW DC9 SRM 51-10-3, 51-10-6 TIMCO REO L-00426 AND DRS 4-999-2.SDR SROM200100022Fitting · corrodedDURING C CHECK INSPECTION AND MAIN LANDING GEAR TIME CHANGE, FOUND FACES OF RT MLG I/B STABILIZER AFT MOUNT FITTING CORRODED. REPLACED FITTING PER MM 57-15-0/SOPM 20-50-01 DWG 65-82770.SDR SWAA010742Fitting · corrodedDURING SCHEDULED D-CHECK AT DALFORT, FOUND RT MLG SUPPORT BEAM STABILIZER BEAM FITTING CORRODED. REMOVED AND REPLACED BEAM FITTING PER MM.SDR SWAA010741Fitting · crackedDURING SCHEDULED D-CHECK AT DALFORT, FOUND RT MLG BEAM ATTACH FITTING. REMOVED AND REPLACED MLG BEAM FITTING PER SWA RA.SDR SROM200100011Beam · corrodedDURING C CHECK INSPECTION, FOUND THE LEFT MLG BEAM HAS SEVERAL AREA OF LEVEL 1 CORROSION ON LOWER SURFACE AT PANEL MOUNTING HOLES.SDR SWAA010674Fitting · corrodedDURING SCHEDULED D-CHECK AT DALFORT, FOUND LT MLG BEAM FITTING CORRODED. REMOVED AND REPLACED BEAM FITTING PER MM.SDR CALA0100186Fitting · crackedINSPECTION FOUND A 1 INCH CRACK IN LT WING MLG SUPPORT BEAM O/B ATTACH FITTING AT AFT SPAR. A NEW FITTING WAS INSTALLED IAW WORK CARD 03-5743-1-0003.SDR SWAA010533Fitting · corrodedDURING SCHEDULED D-CHECK, FOUND LT MLG STABILIZER BEAM FITTING CORRODED AT SUPPORT BEAM. REMOVED AND REPLACED FITTING PER MM.SDR USAA010069Support Fitting · crackedCLT - FOUND FITTING CRACKED .5 INCH, MLG BEAM OUTBOARD SUPPORT FITTING AFT WING SPAR. DEFERRED PER TR 57-40-13. (M)SDR CALA0100078Beam · corrodedINSPECTION FOUND LT WING REAR SPAR LT MLG TRUNNION BEAM STABILIZER FWD LINK CORRODED AT RSS 179.56. REPAIR WAS PERFORMED IAW SRM 51-20-05.SDR SWAA010247Fitting · crackedDURING SCHEDULED D-CHECK AT DALFORT, FOUND LT MLG SUPPORT BEAM FITTING CRACKED. REMOVED AND REPLACED BEAM FITTING PER ACO.SDR SWAA010235Fitting · corrodedDURING SCHEDULED D-CHECK, FOUND RT MLG STABILIZER BEAM FITTING CORRODED. REMOVED AND REPLACED STABILIZER FITTING PER MM.SDR CALA0100046Fitting · crackedINSPECTION FOUND A 1 INCH CRACK IN MLG SUPPORT BEAM O/B SUPPORT FITTING AT LT WING AFT SPAR. THE FITTING WAS REPLACED IAW EA 5743-01022.SDR TWAA0101125Support Fitting · nickedDURING CHECK-C MAINT ON RT WING ON STRUT OF MAIN LANDING GEAR SUPPORT FITTING, THE FWD END OF HYD VALVES HAD A NICK IN THE FITTING. BLENDED OUT NICK PER SRM 53-01 FIG 1 SHEET 1.SDR SWAA010120Fitting · corrodedDURING SCHEDULED SERVICE CHECK, FOUND RT MLG ACTUATOR BEAM SUPPORT FWD FITTING, AT AFT SPAR, CORRODED. REMOVED AND REPLACED FITTING PER MM.SDR SWAA010004Fitting · crackedDURING SCHEDULED 1/4D CHECK, FOUND LT MLG WALKING BEAM FWD OUTBOARD ATTACH LINK CRACKED. REPAIRED FITTING PER SRM.SDR SWA010004Fitting · crackedDURING SCHEDULED 1/4D CHECK, FOUND LT MLG WALKING BEAM FWD OUTBOARD ATTACH LINK CRACKED. REPAIRED FITTING PER SRM.SDR USAA002202Support Fitting · crackedCLT - FOUND MLG BEAM OUTBOARD SUPPORT CRACKED .5 INCH, RT WING AFT SPAR AT WBL 157. REPAIRED PER EA 68723 AND EA 68767. (M)SDR USAA002203Attach Fitting · crackedCLT - FOUND ATTACH FITTING CRACKED .25 INCH, LT MLG SUPPORT BEAM ATTACH FITTING. REMOVED CRACK PER TR 57-40-13. REMOVED CRACK PER TR 57-40-13. (M)SDR SWAA002740Beam · corrodedDURING SCHEDULED SEVICE CHECK, FOUND RT MLG STABILIZER BEAM FWD LUGS CORRODED. R&R STABILIZER BEAM PER MM.SDR SWAA002644Fitting · crackedDURING SCHEDULED D CHECK, FOUND LT WING REAR SPAR UPPER CHORD CRACKED AT MLG BEAM FITTING. REPAIRED MLG FITTING PER EO 00-1248.SDR EF2R2000316Attach Fitting · crackedDURING ROUTINE INSPECTION, LEFT MAIN LANDING GEAR BEAM WING SPAR ATTACH FITTING WAS FOUND CRACKED AT THE SECOND FROM OUTBOARD HOLE. REMOVED AND REPLACED LEFT MAIN LANDING GEAR BEAM WING SPAR ATTACH FITTING.SDR SWAA002484Fitting · crackedDURING SCHEDULED D CHECK AT DALFORT, FOUND RT & LT MLG AFT BEAM FITTINGS CRACKED. R&R BEAM FITTINGS PER ACO 6384-57.SDR EIA2000301Mount · damagedLEFT WING LG INBOARD STRUT MOUNTED DOOR HAS 2 INCH BY 3 INCH DELAMINATION AT LE OF DOOR. REPAIRED PER ECRA 470-52-112-1, PART 1. (M)SDR 2000UALA00691Screw · shearedAFTER REMOVAL OF MLG, DISCOVERED RETAINING SCREWS FOR UPR FWD TRUNNION HOUSING WEAR PLATE SHEARED OFF. *S/D* SCREWS SHEARED DUE TO MLG FORWARD TRUNNION UPPER HOUSING WEAR PLATE MOVEMENT. REPLACED FAILED WEAR PLATE RETENTION SCREWS AND ACCOMPLISHED SERVICE BSDR 20001129SH025Beam · crackedDURING C-CHECK INSPECTION, FOUND A .75 INCH CRACK IN THE WEB AREA AFT SIDE OF THE LEFT MAIN LANDING GEAR SUPPORT BEAM. PART TOTAL TIME AND CYCLES ARE UNKNOWN, BUT AIRCRAFT TT 53,763.0 HOURS. TC: 26,653. (X)SDR ASAA0040125Beam · gougedPAE DURING SCHEDULED MAINTENANCE CHECK, FOUND NR 2 MLG BEAM GOUGED ON THE LOWER SURFACE. FORWARD EDGE, JUST OUTBOARD OF THE JANGER SHAFT FITTING. REPAIRED IN ACCORDANCE WITH EA 5750-01482.SDR DL72L002114Beam · corrodedLT MLG BEAM LOWER FACE CORRODED AT LWR T/E PANEL BORES 2, 5, 6, 7, 8, 9, 11, 12, 14, 15, 28. ALL WORK ACCOMPLISHED PER ERA NR 396313-14, NO REVISION.SDR SWAA002150Support Bracket · corrodedDURING SCHEDULED D-CHECK, FOUND RT WING MLG SUPPORT BEAM CORRODED AT 3 FASTENER HOLES. REPAIRED MLG SUPPORT PER ER 00-1175 AND SRM.SDR DL72L002108Beam · corrodedLT MLG BEAM LWR T/E PNL BORES CORRODED. REAMED HOLES 34, 35, 36, 37 AND 18 TO .312 PER SRM 57-40D. REAMED HOLES 28 AND 39 TO .359 PER SRM 57-40D. REAMED HOLE 32 TO .312 PER SRM 57-40-D. BHEC INSP OF FASTENER FOR CRACKS AND CORROSION. NO ITEM. TURNED O/B SDR DL72L002107Beam · corrodedLT MLG BEAM HOLES BORES NR 2, 5, 6, 7, 8, 9, 11, 12, 14, 15 AND 28 SHOW CORROSION. REAMED HOLES 2, 5 6, 7, 8, 9, 11, 12, 14, 15 TO .312. HOLE 28 TO .359 PER SRM 57-40-D. BHEC INSP OF FASTENERS FOR CRACKS AND COROSION. NO ITEMS. TURNED O/B ON IN PROCESS SDR MWEA001107Fitting · corrodedCORROSION ON FACES OF NR 1 LUG AND NR 2 LUG OF RIGHT MAIN LANDING GEAR TRUNNION. AFT FACE OF NR 1 LUG AND FORWARD FACE OF NR 2 LUG. (LUGS NUMBERED FORWARD AND AFT). REPAIRED NR 1 AND NR 2 LUGS PER TELEX MWX-ORD-00-0385H.SDR SWAA002048Fitting · corrodedDURING SCHEDULED D-CHECK, FOUND LT MLG BEAM STAB LINK FITTING CORRODED. DRILLED STAB LINK FITTING PER DWG 65-82770 AND REPLACED FITTING PER MM.SDR DL733002037Fitting · crackedINSPECTION OF THE RT WING MLG BEAM OUTBOARD ATTACH FITTING REVEALED A CRACK EMANATING FROM A FASTENER HOLE COMMON TO THE REAR SPAR UPPER CHORD. INSPECTION OF THE BOLT HOLE REVEALED TOOLING DAMAGE COMMON TO THE REAR SPAR CAP AND WEB. THE HOLE WAS OVERSIZED TOSDR DL72L002023Beam · corrodedLT MLG BEAM LWR T/E PANEL ATTACH BORES CORRODED. HOLES 35, 29, 27, 26, 25 REAMED TO .312 PER SRM 57-40D. 28 REAMED TO .359 PER SRM 57-40D. REAMED 10 8 TO .312 PER SRM 57-40D. BHEC INSPECT OF FASTENER HOLE FOR CRACKS AND CORROSION. NO ITEM, TURNED O/D ON SDR SWAA002049Fitting · corrodedDURING SCHEDULED D-CHECK, FOUND RT MLG SUPPORT BEAM STAB LINK FITTING CORRODED. REMOVED AND REPLACED LINK FITTING PER MM.SDR DL72L001972Beam · corrodedRT MLG SUPPORT BEAM BORES CORRODED. TASK: C57-581-01.01 FASTENER BORES CORRODED AT HOLES 3, 4, 5, 11, 12, 26, 27, 30, 31, 32, 36 & 38. REWORK HOLES PER DRD 57-40D. 3, 4, 5, 11, 26, 30, 31, 32, 36 REAMED TO 0.358. 27, 12, 13 REAMED TO 0.262. 38 REAMED TO 0SDR SWAA001962Fitting · crackedDURING SCHEDULED 1/2D CHECK, FOUND LT MLG FITTING CRACK EXTENDING FROM UPPER HOLE TO THE EDGE OF THE REAR SPAR CHORD. REPLACED UPPER REAR SPAR CHORD FROM RSS 285 TO THE INBD END PER ER 00-1071.SDR DL72L001963Beam · corrodedAT HMV FOUND RT MLG SUPPORT BEAM BORES CORRODED. FASTENER BORES CORRODED AT HOLES, 17/18/19/22/23/24/39/40/41/42/43/44/45/46. REWORKED CORRODED HOLES PER DRD 57-40D FIG 803D, ALL HOLES ARE 0.312, BHEC INSP OF HOLES LISTED PER DRD 57-40D, SHOWS NO ITEMS.SDR DL72L001962Beam · corrodedAT HMV BHEC OF BEAM NR HOLE 25 ON RMLG SUPPORT BEAM SHOWS CORROSION IN HOLES. REWORK HOLE NR 25 PER DRD 57-40D FIG 803D, NR 25 0.358, BHEC INSP OF HOLE PER DRD 57-40 CKD OK, MECH AND TREATED BUSHINGS PER SRM 57-40D INSTALLED BUSHING PER SRM 57-40D PG 14, STEOSDR EIA2000353Link · corrodedEAC-MZJ - FOUND RIGHT MLG FIXED LINK ATTACH HOLES CORRODED. OVERSIZED HOLES TO REMOVE CORROSION, FABRICATED AND INSTALLED REPAIR BUSHINGS PER ECRA UNIT 57-149-2. (M)SDR EIA2000284Fitting · damagedEAC-MZJ - DURING C6 CHECK, FOUND PREVIOUS BLEND REPAIR RT WING MAIN LANDING SUPPORT FITTING. REPAIRED BLEND REPAIR TO RT WING MAIN LANDING GEAR SUPPORT FITTING, HAND BLENDED, PEENED AND REFINISHED FITTING PER ECRA 944-57-048-2. (M)SDR 20001103SH030Fitting · damagedDURING C-CHECK, FOUND BLEND REPAIR RT WING, MAIN LANDING SUPPORT FITTING. (X)
Back to JASC 5743