JASC 5753
Service difficulty reports · 31,521
Reports filed under 5753 · Trailing Edge Flaps, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5753' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5753' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR EISA98301Skin · delaminatedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD C53-224-01, NINE SMALL AREAS OF DELAMINATION ON RIGHT INBOARD AFT FLAP. REPAIRED ALL AREAS PER SRM 51-40-6. ALUMINUM HONEYCOMB REPAIRS. (M)SDR EISA98297Skin · crackedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD, FOUND AREA WITH GOUGED AND CRACKED SKIN ON UPPER SURFACE OF RIGHT INBOARD AFT FLAP. REMOVED DAMAGED SKIN. FABRICATED AND INSTALLED NEW SKIN SECTION PER SRM 57-50-4. (M)SDR EISA98288Skin · delaminatedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD, FOUND THREE AREAS OF DELAMINATION ON RIGHT INBOARD MID FLAP TRAILING EDGE. REPAIRED AREAS PER SRM 51-40-6 ALUMINUM HONEYCOMB REPAIR. (M)SDR EISA98287Skin · puncturedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD, FOUND SKIN PUNCTURE ON RIGHT INBOARD MID FLAP TRAILING EDGE LOWER SIDE. REPAIRED SKIN PUNCTURE PER SRM 51-40-6, 51-40-8, AND 51-40-9. (M)SDR EISA98285Skin · delaminatedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD, FOUND TWO AREAS OF DELAMINATION ON LEFT INBOARD MID FLAP. REPAIRED AREAS OF DELAMINATION PER SRM 51-40-6 AND 51-40-8. (M)SDR AU981637Flap · malfunctioned(AUS) ON LANDING, THE RT OUTBOARD TE FLAPS STOPPED AT 25 DEGREES. FURTHER ATTEMPTS TO DRIVE FLAPS RESULTED IN STALLED DRIVE ABILITY. INVESTIGATION FOUND A SHEARED FITTING BETWEEN THE FLAP AND FLAP-DRIVE BALLSCREW.SDR SWIA971335Flap · damagedFLAP DISAGREEMENT ON FLAP RETRACTION RIGHT SIDE. RETURNED TO SLC. REMOVED AND REPLACED LEFT OUTBOARD FLAP IAW EMB MM 27-50-04, OPS CHECKS GOOD.SDR P5CA9801619Skin · holeLEFT WING OUTBOARD POSITION FORE FLAP LEADING EDGE HAS HOLE IN PREVIOUS REPAIR. REPAIRED DAMAGED AREA PER SRM 51-40-09.SDR DL72L990175Spar · crackedAFT SPAR RAIL LWR CHORD ANGLE CRACKED 2 PLACES 19 AND 23 FROM I/B END. REPAIRED PER M/M 57-52-0 FIG 802, ON SHOP ORDER 634487.SDR DL72L990174Spar · crackedAFT SPAR RAIL LWR CHORD ANGLE CRACKED 2 PLACES 32 AND 37 FROM I/B END. REPAIRED PER M/M 57-52-0 FIG 802, ON SHOP ORDER 634487.SDR DL72L990173Spar · crackedAFT SPAR RAIL LWR CHORD ANGLE CRACKED 61 FROM I/B END. REPAIRED PER M/M 57-52-0 FIG 802, ON SHOP ORDER 634487.SDR TWAA9819809Skin · delaminatedDURING OP 15 MAINT CHECK, FOUND RT WING LOWER SIDE APPROX 40 INCHES I/B OF O/B END, HAS 8 INCH BY 3 INCH DELAMINATION ON RT FLAP, O/B END. REMOVED OLD EXISTING REPAIR AND REPLACED WITH PRE-PREG FIBERGLASS PER SRM 57-53-01, TABLE I, FIG 201 (SHEET 5), SRM 51-7SDR 99ZZZX421Spar · corrodedCORROSION ON AILERON AND FLAP SPARS.SDR ABXA9801140Bracket · corrodedDURING C-CHECK, FOUND LEFT FLAP INBOARD AFT HINGE BRACKET CORRODED AT PIVOT POINT. REPLACED AFT HINGE BRACKET IAW DC9 SRM.SDR ABXA9801136Fitting · crackedDURING C-CHECK, FOUND LEFT FLAP INBOARD FIXED VANE OUTBOARD ATTACH SUPPORT FITTING BROKEN. REPLACED FITTING IAW DC9 SRM 51-30-2, 52-30-5, AND DACO DWG 9957773.SDR QXEA9801905Track · corrodedLIGHT CORROSION TO MLG BEAM BOLT HOLES, SPOILER BEAM BOLT HOLES, AND AFT MLG DOOR HINGE FITTING BOLT HOLES. REAMED HOLES TO REMOVE CORROSION. MLG BEAM BOLT HOLES OVERSIZED AND LEFT AS-IS. SPOILER BEAM BOLT HOLES BUSHED. AFT MLG DOOR HINGE FITTING BOLT HOLESDR MZZA98289Flap Track · corrodedTNN - DURING D-CHECK INSPECTION ON AIRCRAFT AT AIR ASIA, CORROSION WAS FOUND ON NR 4 FLAP TRACK MOUNTING PAD 'A' AROUND THE BOLT HOLE. THE DAMAGED NR 4 FLAP TRACK P/N 65-19270-10 WAS REMOVED AND REPLACED PER B727 MM 27-51-31. (M)SDR DHL9872061DFlap · damagedAT D CHECK, LEFT I/B MID FLAP DAMAGED AT I/B AFT END. INSTALLED F/G OVERLAY PER SRM 51-40-8, 5 BY 8 N/R 1084.SDR TWAA9819103Skin · delaminatedDURING CHECK-C MAINT, FOUND LT WING O/B FLAP, LOWER SURFACE AT I/B END, WITH DELAMINATION APPROX 12 IN BY 27 IN. APPLIED 28 IN BY 16 IN HOT BOND REPAIR PER SRM 57-53-01 AND SRM 51-70-05.SDR MZZA98291Angle · crackedTNN - DURING D-CHECK INSPECTION ON AIRCRAFT AT AIR ASIA, 1.125 INCH LONG CRACK WAS FOUND ON RT WING T/E INBOARD MID FLAP LOWER CLOSURE ANGLE AT WBL 124. THE CLOSURE ANGLE CRACK AREA (1.125 INCH LONG) WAS TRIMMED OUT AND REPAIRED PER B727 SRM 51-40-4. (M)SDR ABXA9801144Fitting · crackedDURING C-CHECK, FOUND LEFT FLAP OUTBOARD HINGE INTERNAL ATTACH FITTING CRACKED. REPLACED FITTING IAW DC9 SRM 51-30-1 AND 51-30-2.SDR CKSA98693Plate · corrodedRT TRAILING EDGE FLAP TRACKS 1, 2, 3, SIDE LOAD SURFACES (UPPER INBD AND AFT OUTBD) CORRODED BEYOND LIMITS. REPAIRED IAW BOEING ASA CKF-EXW-132 SUPP SHT 1, 2, 3. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASSDR CKSA98692Web · corrodedRT OUTBD T/E MIDFLAP NR 3 SPAR WEB AT CENTER OF FLAP HAS 2 AREA OF CORROSION BEYOND LIMITS. REPAIRED WEB IAW BOEING ASA CKF-EXW-135. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CARDS AT BOEING WICHITA (KISDR CKSA98691Track · pittedFLAP TRACK NR 5 RT, ZONE 600, WING TO TRACK MATING SURFACE PITTED BEYOND LIMITS. REPAIRED IAW BOEING ASA CKF-EXW-130 SUPP SHT 1, OHM 57-52-70 REPAIR 6-1, S/B 747-57-2207 FIG 1; NOTES 5, 12, 13 AND OHM 57-52-70 REPAIR 1-1, PARA 1C & 1E. FOUND DURING ACCOMPLISSDR CKSA98690Track · corrodedRT WING FLAP TRACKS NR 6, 7, 8, ZONE 600, BUSHING MOUNT HOLES CORRODED. REWORKED BUSHING MOUNTS IAW BOEING ASA CKF-EXW-117 SUPP SHT 1. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CARDS AT BOEING WICHITA (SDR CKSA98689Track · corrodedZONE 500, NR 1 LT FLAP TRACK BUSHING FWD BOLT HOLES AND MOUNTING AREA CORRODED BEYOND LIMITS. REPAIRED IAW BOEING ASA CKF-EXW-108 SUPP SHT 1. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CARDS AT BOEING WISDR CKSA98688Track · corrodedZONE 500, NR 4 LT FLAP TRACK BUSHING FWD BOLT HOLES AND MOUNTING AREA CORRODED BEYOND LIMITS. REPAIRED IAW BOEING ASA CKF-EXW-083 SUPP SHT 2. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CARDS AT BOEING WISDR CKSA98687Tie Plate · corrodedLT I/B MIDFLAP ZONE 500, WBL 216 LT, AN AREA 5 X 1.5 INCH OF EXFOLIATED CORROSION EXISTS ON LWR I/B SFC. REPAIRED IAW BOEING ASA CKF-EXW-115 SUPP SHT 1 AND 2. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CSDR CKSA98686Plate · rustedRT FLAP TRACK NR 5, ZONE 600, MOUNTING PLATE SEVERE RUST FOUND. REPAIRED IAW BOEING ASA CKF-EXV-071 SUPP SHT 2. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OF CPCP TASK CARDS AT BOEING WICHITA (KIAB). WORK ORDER NUMBSDR CKSA98685Plate · corrodedRT WING FLAP TRACK BEARING PLATES AT STA 353 WBL 584 AND 743 (NR 5, 6, 7) SHOW MODERATE CORROSION. REPLACED PLATES IAW BOEING DWG 65B07782 AND ASA CKF-EXW-072 SUPP SHT 2. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECK, AND ACCOMPLISHMENT OFSDR CKSA98684Skin · corrodedRT AFT I/B TRAILING EDGE FLAP UPPER SKIN ON O/B PANEL HAS 5 EXISTING PATCHES NOT DONE IAW SRM REQUIREMENTS. PEELING, CORROSION AND SEPARATING WERE REPAIRED IAW BOEING ASA CKF-EXW-010 SUPP SHT 2. FOUND DURING ACCOMPLISHMENT OF CARGO CONVERSION, ROUTINE C-CHECSDR MZZA98290Skin · delaminatedTNN - DURING D-CHECK INSPECTION ON AIRCRAFT AT AIR ASIA, DELAMINATION WAS FOUND ON LEFT WING T/E INBOARD MID FLAP UPPER SKIN AT WBL 226. THE DAMAGED SKIN 7 INCH BY 2 INCH IN SIZE WAS TRIMMED OUT AND REPAIRED PER B727 SRM 51-40-6. (M)SDR AU981627Track · damaged(AUS) RIGHT FLAP TRACK MUSHROOMED AND TORE THE ROLLER SPACER, JAMMING THE ROLLER P/N 0523920 AND CAUSING THE FLAP TO JAM. THE FLAP MOTOR CONTINUED TO DRIVE UP AND TWISTED THE FLAP.SDR CALA9802079Skin · dentedINSPECTION FOUND LT I/B TE FOREFLAP DENTED AND A 1 X 1 AREA OF DEBONDING JUST OUTBOARD OF NR 3 FLAP TRACK AREA AT LOWER SURFACE. THE LT I/B TE FOREFLAP WAS REMOVED AND REPLACED IAW MM 27-51-1.SDR CALA9802071Plate · crackedINSPECTION FOUND A 1 INCH CRACK IN PLATE AT RT INBOARD MIDFLAP ABOVE AFT END OF NR 5 SPINDLE. THE PLATE WAS REMOVED IAW SRM 51-30-2, PAGE 4. A NEW PLATE WAS INSTALLED IAW SRM 51-10-1 AND 51-10-2, PAGE 1.SDR ASAA9880236Fitting · gougedLCQ - DURING 30K CHECK, GOUGES WERE FOUND ON LEFT T/E FLAP OUTBOARD HINGE FITTING. REPAIRED IAW ASA EA 2750-01066. (M)SDR DHL9980170CFitting · crackedAT C-CHECK, RIGHT WING FLAP HINGE FITTING BOLT HOLE NR 3A LEFT CRACKED. REMOVED AND REPLACED FITTING PER SRM 51-1-2.SDR COMA9860351Skin · chafedRIGHT HAND FLAP LEADING EDGE HAS CHAFE DAMAGE. REPLACED LEADING EDGE.SDR MZZA98292Angle · crackedTNN - DURING D-CHECK INSPECTION ON AIRCRAFT AT AIR ASIA, 2 INCH LONG CRACK WAS FOUND ON RT WING T/E INBOARD MID FLAP LOWER CLOSURE ANGLE AT WBL 204. THE CLOSURE ANGLE CRACK AREA (2 INCH LONG) WAS TRIMMED OUT AND REPAIRED PER B727 SRM 51-40-4. (M)SDR EISA98260Skin · delaminatedROUTINE C-CHECK WORK CARD ACCOMPLISHMENT REVEALED LEFT INBOARD T/E FLAP DELAMINATED AT OUTBOARD CORNER. REPAIRED DELAMINATION PER SRM 51-40-5, BONDED METAL REPAIR. (M)SDR EISA98274Skin · delaminatedDURING ACCOMPLISHMENT OF ROUTINE C-CHECK WORK CARD FOUND RIGHT INBOARD MID FLAP DELAMINATED. REPAIRED MID FLAP PER SRM 51-40-6. (M)SDR QXEA01766Tracks · corrodedLEFT-HAND NR 1 AND RIGHT-HAND NR 2 FLAP TRACKS HAVE PITTING CORROSION ON BACK SIDE OF TRACK. REPAIRED IAW DHC-8 RD 8-57-1282.SDR CA981123024Support · failed(CAN) RIGHT FLAP FAILED. INSP FOUND OUTER SECTION OF INBD FLAP SUPPORT ARM P/N 0522901-14 HAD FAILED 2 INCHES AFT OF FORWARD BOLT HOLE. THE INNER SECTION OF INBD FLAP SUPPORT ARM P/N 0523901-13 HAD FAILED JUST AFT OF BOLT HOLE. METAL DISCOLORED. CRACK FOUSDR TWAA9818407Skin · delaminatedDURING CHECK-C MAINT, FOUND ON RT WING THE TRAILING EDGE FLAP TOP SIDE OF I/B TRAILING EDGE FLAP AT O/B END WAS DELAMINATED APPROX 2 FT IN FROM O/B END. INSTALLED 9 IN BY 12 IN METAL HOT BONDED DOUBLER PER SRM 57-53-01 AND 57-70-10.SDR DL72S982322Skin · crackedA .375 INCH CRACK AT NR 2 MIDFLAP LOWER SURFACE AT CUTOUT I/B OF NR 4 MIDFLAP FAIRING. REPAIRED PER M/M 57-52-0.SDR DHL9872092DCasting · crackedAT D CHECK, RT O/B FOREFLAP I/B END CASTING CRACKED AT FWD L/E RADIUS. REMOVED AND REPLACED CRACKED CASTING PER SRM 57-50-1, N/R 2893.SDR QXEA9801882Track · corrodedPITTING CORROSION IN THE UPPER PORTION OF THE FLAP TRACK AT STATION 1700. REPAIRED IAW FOKKER SRM 51-10-04.SDR QXEA9801689Skin · damagedLEFT-HAND INBOARD FLAP LOWER INBOARD TRAILING EDGE HAS LARGE AREAS OF ROCK DAMAGE FROM MAIN TIRES. REPAIRED IAW FOKKER SRM 51-20-0, PARAGRAPH 4.SDR CALA9802049Skin · dentedINSPECTION FOUND THE LT OUTBOARD TRAILING EDGE FLAP INBOARD SKIN DENTED AT LOWER FLAP 29 INCHES FROM INBOARD END. THE DENTED AREA WAS TRIMMED OUT AND REINFORCED WITH DOUBLER IAW SRM 57-10-00, FIGURE 7, 51-21-01, AND 51-31-01.SDR AU981458Shoe · loose(AUS) FLAP DISAGREEMENT. INVESTIGATION FOUND A FLAP BONDING SHOE DISPLACED AND LOADING THE LT OUTBOARD FLAP TRACK.
Back to JASC 5753