Boeing MD-11F
Service difficulty reports · 31,322
Newest first. General aviation reporting is voluntary.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = 'MD11F' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = 'MD11F' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR 08FDEA02099None · noneEXISTING DOUBLER REPAIR AT FORWARD CARGO DOOR FORWARD CUT-OUT APPROX STRINGER 38 TO 42. EXISTING DOUBLER REPAIR AT FORWARD CARGO DOOR FORWARD CUT-OUT APPROX. STRINGER 38 TO 42 EVALUATED AND FOUND PREVIOUSLY ACCOMPLISHED AS PER SRM 53-50-00 FIGURE 17 VOLUME ISDR 08FDEA02098None · noneEXISTING DOUBLER REPAIR AT RIGHT FUSELAGE APPROX STA 1019 TO STA 1039, STRINGER 40 TO 43. EXISTING DOUBLER REPAIR AT RIGHT FUSELAGE APPROX STA 1019 TO STA 1039, STRINGER 40 TO 43 EVALUATED AND FOUND PREVIOUSLY ACCOMPLISHED AS PER SRM 53-20-00 FIGURE 10 VOLUMESDR 08FDEA02097None · noneEXISTING DOUBLER REPAIR AT RIGHT FUSELAGE APPROX STA 2003 TO STA 2004, STRINGER 38 TO 41. EXISTING DOUBLER REPAIR AT RIGHT FUSELAGE APPROX STA 2003 TO STA 2004, STRINGER 38 TO 41 EVALUATED AND FOUND PREVIOUSLY ACCOMPLISHED PER SRM 53-20-00 FIGURE 2 VOLUME ISDR 08FDEA02084Skin · corrodedUPON AFT FUSELAGE RT LOWER WASTE VACUUM EXHAUST PLUG REMOVED AT STA 1959 BETWEEN LONGERON 39R TO 40R, FOUND EXISTING DOUBLER CORRODED. AFT FUSELAGE RT LOWER, AT STA 1959 BETWEEN LONGERON 39R TO 40R REPAIR CARRIED OUT AS PER SRM 53-20-00 VOL 1 FIG 2. REPAIRSDR 08FDEA02082Skin · crackedCRACK FOUND QUANTITY 13 FASTENER HOLES ON RT SIDE LOWER SKIN PANEL OUTER WING ACCESS DOOR CUT-OUT BETWEEN STA XORS=683.4 AND XORS=713.6 RT SIDE LOWER SKIN PANEL OUTER WING ACCESS DOOR CUT-OUT BETWEEN STA XORS=683.4 AND XORS=713.6 13 FASTENER HOLES CRACKED. ARSDR 08FDEA02081Skin · crackedCRACK FOUND QUANTITY 3 FASTENER HOLES ON LT SIDE LOWER SKIN PANEL OUTER WING ACCESS DOOR CUTOUT BETWEEN STA XORS=683.4 AND XORS=713.6. LT SIDE LOWER SKIN PANEL OUTER WING ACCESS DOOR CUTOUT BETWEEN STA XORS=683.4 AND XORS=713.6 03 FASTENER HOLES CRACKED. AREASDR 08FDEA02080Fitting · crackedDURING HFEC OPEN HOLE INSPECTION ON LOWER JAMB SUPPORT FITTING BOLT BORE HOLE, 01 EA CRACK WAS FOUND ON THE FWD SIDE OF 3RD LAYER ON THE AFT I/B BOLT HOLE AT NR 7 LOWER JAMB SUPPORT FITTING. CRACKED LOWER JAMB NR 7 SUPPORT FITTING REMOVED AND REPLACED AS PER SDR 08FDEA02083Frame · crackedCAC COMPARTMENT AT STA 1139 LONGERON 29L TO 30L FRAME SPLICE FOUND CRACKED.SDR UPS08M52855Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR 31 FOUND CORRODED CORROSION AT BARREL NUT BORE REMOVED IAW SRM 51-21-01 VII REV35.BORE REAM TO 1.162"DIA, REMAINING BLEND OUT AT BOTTOM RADIUS 0.130" DEEP FOUND EXCEEDING EO LIMIT IAW EO MD11-5510-19409M.SDR UPS08M52853Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR34 FOUND CORRODED EXISTING SLEEVE BUSHING REMOVED & CORROSION AT BARREL NUT BORE REMOVED IAW SRM 51-21-01 VII REV 35. BORE REMAINING BLEND OUT 0.030" DEEP, BOTTOM SURFACE CLEANED, BORE BLEND OUT EXCEEDED SDR UPS08M52396Pump · leakingINSPECTION TYPE:N/A ATB - NR 2 HYDRAULIC FAIL ALERT MESSAGE. EMERGENCY DECLARED. FOUND NR 2 ENGINE L FWD HYD PUMP LEAKING FROM CASE DRAIN. REMOVED AND REPLACED NR 2 ENG LT & RT HYDRAULIC PUMPS AND FILTERS.SDR UPS08M52850Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR 28 FOUND CORRODED, CORROSION AT BARREL NUT BORE REMOVED IAW SRM 51-21-01 VII REV35. BORE REAMED TO 1.178" DIA, REMAINING BLEND OUT 0.060", BOTTOM REMAINING 0.070" DEEP. BORE BLEND OUT FOUND EXCEEDING LIMISDR 08FDEA02005Stanchion · corrodedFORWARD CARGO COMPARTMENT: AFTER REMOVAL OF STA 6-73 AFT BULKHEAD PANEL FOR WIRING INSPECTION ACCESS FOUND X = 57 STANCHION WITH CORROSION. CORRODED STANCHION AT STA 6-73, X = 57 AFT BULKHEAD PANEL REMOVED AND REPLACED AS PER SRM 51-31-01 VOLUME II. STANCHIOSDR 08FDEA02004Stanchion · corrodedFORWARD CARGO COMPARTMENT: AFTER REMOVAL OF STA 6-73 AFT BULKHEAD PANEL FOR WIRING INSPECTION ACCESS FOUND X = 30 STANCHION WITH CORROSION. CORRODED STANCHION AT FWD CARGO COMPARTMENT AFT BULKHEAD STA 6-73; X=30. REMOVED AS PER SRM 51-31-01 VOL II. NEW STANSDR 08FDEA02003Stanchion · corrodedAFTER REMOVAL OF FORWARD CARGO AFT BULKHEAD STA 6-70 PANEL FOR WIRING INSPECTION FOUND PANEL SUPPORT APPROXIMATELY 10 INCH RIGHT FROM CENTER FOUND CORRODED. CORRODED STANCHION AT FORWARD CARGO AFT BULKHEAD STA 6-70 10 INCH RIGHT FROM CENTER REMOVED AND REPLSDR 08FDEA02002Stanchion · corrodedAFTER REMOVAL OF FORWARD CARGO AFT BULKHEAD STA 6-70 PANEL FOR WIRING INSPECTION FOUND PANEL SUPPORT LEFT 10 INCH FROM CENTER FOUND CORRODED. FORWARD CARGO AFT BULKHEAD STA 6-70 LEFT X = 9.05 STANCHION REMOVED AND REPLACED AS PER SRM 51-31-01 VOLUME II. SDR 08FDEA02011Skin · crackedRT WING LEADING EDGE ANTI-ICE TELESCOPIC DUCT CUT-OUT TOP INBOARD AND OUTBOARD CORNER FOUND CRACKED. REPAIR CARRIED OUT AS PER SRM 57-10-00, REPAIR CLASSIFIED MAJOR AS PER GMM 6-2-100.SDR 08FDEA02010Frame · dentedAFT CABIN AT APPROXIMATELY STATION 1721 LEFT SIDE LONGERON 12 LEFT FOUND FRAME DENTED. CARRIED OUT REPAIR AS PER SRM 53-30-00, REPAIR CLASSIFIED MAJOR AS PER GMM 6-2-100.SDR 08FDEA02009Frame · dentedAFT CABIN AT APPROXIMATELY STATION 1761 LEFT SIDE LONGERON 12 LEFT FOUND FRAME DENTED. BS 1761 LT LONGERON 12 LT FRAME CARRIED OUT REPAIR AS PER SRM 53-30-00, FIG.1, VOL.I. DUE TO CAT B REPAIR, INITIAL INSPECTION TO BE CARRIED OUT AT 14,500 CYCLE, WITH REPETSDR 08FDEA02008Frame · dentedAFT CABIN AT APPROXIMATELY STATION 1701 RIGHT SIDE LONGERON 12 RIGHT TO LONGERON 13 RIGHT FOUND FRAME DENTED. AFT BS 1701 FRAME RT LONGERON 12 TO 13 RT CARRIED OUT REPAIR AS PER SRM 53-30-00, FIG.1, VOL.I. DUE TO CAT B REPAIR, INITIAL INSPECTION TO BE CARRSDR 08FDEA02007Doubler · crackedLEFT WING, LEADING EDGE RIB DOUBLER AT XOS 667 FOUND CRACKED. REMOVED CRACKED RIB DOUBLER AS PER SRM 51-31-01, VOL. II. FABRICATED NEW RIB DOUBLER AS PER DRAWING ARB3954. INSTALLED NEW RIB DOUBLER AT LT WING LEADING EDGE AT XOS 667 AS PER SRM 51-33-01, VOSDR 08FDEA02006Skin · crackedLEFT WING ANTI-ICE TELESCOPIC DUCT DOOR CUT OUT CORNER FOUND CRACKED AT STATION XOS 464 AND XOS 470. REPAIR CARRIED OUT AS PER SRM 57-10-00, FIG.43, VOL.I AND EA 1-5710-122715, REPAIR CLASSIFIED MAJOR AS PER GMM 6-2-100.SDR UPS08M52844Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR 8 FOUND CORRODED CORROSION REMOVED AT BARREL NUT BORE IAW SRM 51-21-01 VII REV 35. BORE REAM TO 0.988" DIA REMAINING BLEND OUT 0.095" DEEP, BOTTOM SURFACE CLEANED. BORE BLEND OUT FOUND EXCEEDING LIMITS SDR UPS08M52854Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR17 FOUND CORRODED. CORROSION REMOVED AT BARREL NUT BORE IAW SRM 51-21-01 VII REV35. BORE REAM TO 1.067"DIA, REMAINING BLEND OUT 0.050", BOTTOM REMAINING, BLEND OUT 0.045" DEEP, FOUND EXCEEDING LIMIT IAW SDR 08FDEA01982Door Frame · corrodedAFT CARGO COMPARTMENT, AFTER REMOVAL OF DAMAGED DOOR CUT-OUT AFT LOWER SCUFF PLATE FOUND DOOR JAMB STRUCTURE WITH CORROSION. REPAIR CARRIED OUT AS PER FEDEX EA 1-5310-122464, REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR UPS08M52845Structure · corrodedINSPECTION TYPE-C, LT HORIZ STAB BARREL NUT BORE NR33 FOUND CORRODED CORROSION AT BARREL NUT BORE REMOVED IAW SRM 51-21-01 VII REV 35. BORE REAM TO 1.178" DIA, REMAINING SIDEWALL BLEND OUT 0.020" DEEP, BOTTOM SURFACE REMAINING BLEND OUT 0.065" DEEP, BLENSDR UPS08M52842Structure · corrodedINSPECTION TYPE-C, LT HORIZ STAB BARREL NUT BORE NR17 FOUND CORRODED. CORROSION AT BARREL BORE REMOVED IAW SRM 51-21-01 VII REV 35. BORE REAM TO 1.067" DIA REMAINING BLEND OUT 0.035", BOTTOM SURFACE CLEANED & BORE FOUND OUT OF LIMIT IAW EO MD11-5510-194SDR UPS08M52372Doubler · crackedINSPECTION TYPE:2C HAIRLINE CRACK 2 PLACES ON RT WING TOP OF ANTI-ICE TELESCOPIC DUCT CUT OUT CORNER. REMOVED DAMAGE IN 2 PLACES, FABRICATED FILLERS AND DOUBLER AND INSTALLED IAW MD-11 SRM 57-10-00, 51-31-01, AND 51-21-01F.SDR WRLA2008050Doubler · corrodedFOUND FUSELAGE WASTE SERVICE PANEL EXTERNAL DOUBLER CORRODED STA Y392.00 TO STA Y421.507 CENTER LINE. DOUBLER REPLACED PER SRM 51-30-00 VOL 2 REV 40.SDR UPS08M52365Light · inoperativeINSPECTION TYPE:N/A 2 BULBS NOT ILLUMINATED OVER LT ENTRANCE DOOR DURING EMERGENCY LIGHT TEST. RELAMPED EMERGENCY LIGHTS, OPS CHECK NORMAL.SDR UPS08M52848Structure · corrodedINSPECTION TYPE-C, RT HORIZ STAB BARREL NUT BORE NR 36 FOUND CORRODED CORROSION AT BORE NR36 RT REMOVED IAW SRM 51-21-01 VII REV 35. BORE REAM TO 2.538" DIA, REMAINING BLEND OUT 0.098" DEEP, BOTTOM REMAINING BLEND OUT 0.150" DEEP, BORE EXCEEDED LIMITS IASDR UPS08M52374Fitting · crackedINSPECTION TYPE:2C RT WING L/E FITTING HAS CRACKED APPROX 1 INCH BETWEEN NR 1 AND NR 2 L/E SLAT. REMOVED, FABRICATED, AND INSTALLED FITTING IAW DWG ARB1602, MD-11 SRM 51-31-01.SDR UPS08M52373Longeron · corrodedINSPECTION TYPE:2C CENTER CARGO COMP BILGE AREA FOUND CORROSION AT STA 5-53 TO 5-123 LONGERON 47RH AS MARKED. REMOVED CORRODED LONGERON AND SPLICE, FABRICATED LONGERON AND SPLICE AND INSTALLED IAW SAA TRAVELER 79724800001, 797244810001, AND DWG ASA 7031 AND MSDR UPS08M52371Doubler · damagedINSPECTION TYPE:2C DOUBLER IS PEELED BACK AFT OF RADOME ON TOP. REMOVED DOUBLER, CUTOUT CRACK, FABRICATED FILLER AND DOUBLER AND INSTALLED IAW MD-11 SRM 51-31-01, 53-00-01, 53-35-01 NS 51-21-02.SDR UPS08M52451Structure · crackedINSPECTION TYPE:2C LT WING OUTBOARD L/E FIXED PANEL, SLAT ANTI-ICE DUCT ACCESS CUTOUT AREA FOUND UPPER CORNER CRACKED. CUT OUT TWO EACH AREAS, FABRICATED 2 EA DOUBLERS AND FILLERS, AND INSTALLED IAW MD11 SRM 57-10-00, 51-35-01, 51-21-01, AND 51-21-02.SDR 08FDEA01956Trunnion · crackedNLG LT TRUNNION FITTING FWD EDGE FOUND WITH CRACK. REPAIRED AS PER SRM 53-40-00 FIGURE 23 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100. REPETITIVELY INSPECT FOR CRACK GROWTH AT NOT TO EXCEED 1,500 LANDING INTERVALS IN REFERENCE TO WITH SRM 53-40-00 SDR UPS08M52450Stringer · crackedINSPECTION TYPE:2C LT WING L/E FIXED PANEL SUPPORT LOWER STRINGER FOUND CRACKED AT WING STA YORS AS MARKED, JUST O/B OF SLAT DRIVE MECHANISM. FABRICATED AND INSTALLED DOUBLER IAW MD11 SRM 57-10-00 FIG 18, 51-31-01, AND 51-21-01.SDR UPS08M52449Strap · crackedINSPECTION TYPE:2C RIGHT WING L/E SPLICE STRAP XFS 669 CRACKED. REMOVED, FABRICATED, AND INSTALLED SPLICE STRAP IAW MD11 SRM 51-21-01, 51-33-01, AND DWG ARB3954.SDR 08FDEA01927Longeron · crackedCRACK INDICATION FOUND DURING X-RAY INSPECTION AT STA 6-100, LONGERON 2L, FORWARD SECTION EDGE, CRACK LENGTH APPROX 1 INCH. REPAIRED AS PER SRM 53-10-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01926Longeron · crackedCRACK INDICATION FOUND DURING X-RAY INSPECTION AT STA 6-0, LONGERON 2L, AFT SECTION EDGE, CRACK LENGTH APPROX 1.5 INCH. REPAIRED AS PER SRM 53-10-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01925Longeron · crackedCRACK INDICATION FOUND DURING X-RAY INSPECTION AT STA 6-100, LONGERON 1R AFT SECTION EDGE, CRACK LENGTH APPROX 0.5 INCH. REPAIRED AS PER SRM 53-10-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01924Frame · dentedMAIN DECK TRANSVERSE FRAME REPAIR AT STA 1701 L=12R FOUND DENTED. REPAIRED AS PER SRM 53-30-00 FIGURE 1 VOLUME I. INITIAL INSPECTION REQUIRED AT 14,500 CYCLES AND REPETITIVE INSPECTION AT EVERY 9,500 CYCLES TO BE CARRIED OUT AS PER SRM 53-30-00 FIGURE 1 VOLSDR UPS08M53521Spar · corrodedINSPECTION TYPE:N/A VERTICAL STABILIZER FRONT SPAR RT AT STA ZFS 353.295 FOUND SURFACE CORROSION. SURFACE CORROSION ON VERTICAL STABILIZER FRONT SPAR RT AT STA ZFS 353.295 REMOVED AS PER SRM 51-21-01 VOL II REV 35. REWORKED AREA MATERIAL ORIGINAL THICKNESS 0SDR 08FDEA01888Skin · dentedRT WING INBD FLAP LOWER SURFACE FOUND WITH 3 DENT MARKS AT XIFH 249. DENTS ON RIGHT HAND WING INBD FLAP LOWER SURFACE AT XIFH 249 MEASURED AND FOUND OUT OF LIMITS AS PER SRM 57-10-00 FIGURE 17 VOLUME I. REPAIR CARRIED OUT AS PER SRM 57-10-00 FIGURE 3 VOLSDR UPS08M52448Skin · crackedINSPECTION TYPE:2C RIGHT WING OUTER ACCESS PNL LANDING HAS CRACK. CRACK BETWEEN UPPER AND LOWER HINGE. VIEWED WITH MIRROR. FABRICATED AND INSTALLED REPAIR DOUBLER IAW MD11 SRM 57-10-00 FIG 18.SDR UPS08M52545Longeron Splice · crackedINSPECTION TYPE:C CTR CARGO AT STATION 1676 LONGERON 46 RT LONGERON SPLICE DOUBLER FOUND CRACKED AS MARKED. CRACK SPLICE REMOVED PER SRM 51-33-01 VII REV 35. REPAIR LONGERON SPLICE FAB PER SRM 53-10-00 FIG 2 VI REV 35. NEW SPLICE REWORKED SMOOTH AND REPROTESDR 08FDEA01896Skin · misrepairedEXISTING DOUBLER REPAIR AT FWD CARGO DOOR AFT CUT-OUT AT APPROX STR 39-42 NOT IAW SRM STANDARDS. EXISTING REPAIR AND FOUND NOT IAW. SRM 53-50-00 FIG 17 VOL. I. REPAIR CARRIED-OUT AS PER SRM 53-50-00 FIG. 17 VOL. I. REPAIR CLASSIFIED AS MAJOR AS PER GMM 6-2-SDR 08FDEA01895Fitting · crackedMAIN DECK CARGO DOOR SPOOL FITTING NR 7 FOUND 3RD LAYER CRACK INDICATION AT FITTING BOLT HOLES 'A', 'B', 'C' AND 'D'. FITTING REMOVED AND REPLACED AS PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01894Fitting · crackedMAIN DECK CARGO DOOR SPOOL FITTING NR 6 FOUND 3RD LAYER CRACK INDICATION AT FITTING BOLT HOLES 'A' AND 'D'. FITTING REMOVED AND REPLACED AS PER SRM 51- 31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01893Fitting · crackedMAIN DECK CARGO DOOR SPOOL FITTING NR 5 FOUND 3RD LAYER CRACK INDICATION AT FITTING BOLT HOLE 'C'. FITTING REMOVED AND REPLACED AS PER SRM 51-31 -01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.
Back to Boeing MD-11F