What was found
RT RUDDER SKIN OIL CANNING (STA ZR 136.000 - 125.000) MAJOR REPAIR. PERFORMED MAJOR REPAIR IAW SRM 55-6-1 FIG 1. REMOVED DAMAGED PANEL PLATING IAW SRM 55-1-0 PG 1, SRM 51-1-21. FABRICATED PLATING AND BONDED DOUBLER BOTH FROM AL2024T3 0.016" IAW SRM 55-6-1 FIG 1 ITEM "A". BONDED BOTH PARTS WITH HYSOL IAW SRM 51-1-9, TR NR 51-142, SRM 51-1-9A, TR NR 51-141. CLEANED, TREATED AND PRIMED AREA AND PANEL PLATING IAW SRM 51-1-8B. INSTALLED PANEL PLATING IAW SRM 51-1-11, SRM 51-1-21, SRM 51-1-21A. REFER TO NR 107097 FOR BALANCING.