What was found
CABIN HAS CHORD CRACKED AT END RADIUS BS 312 S5L-S6L. / CUT OUT DAMAGE AT CABIN CHORD AT END RADIUS BS 312 S5L-S6L; PERFORMED HFEC AND ROTO INSP NO CRACK NOTE AS PER NTM PART 6 51-00-00 PROCEDURE 23; FABRICATED ANGLE REPAIR MAT USED 7075-0 0.063 CLAD PO #1668003; PERFORMED HEAT TREAT; CONDUCTIVITY AND HARDNESS INSP AS PER BAC5946 FOUND IN LIMITS; DRILLED; DE-BURRED; TREAT; PRIMER AND INSTALLED REPAIR PART AS PER REF B737-700 SRM 53-10-07-2R-1 FIG A REPAIR 1; PERFORMED FPI SOPM 20-20-02; SRM 51-40-05-0G-0; AMM 51-21-41-701; AMM