What was found
CABIN FLOOR PANEL 232RF FORWARD CORNER DELAMINATED (DOT 6) ; / [01] EVALUATED AND FOUND DAMAGE TO UPPER SURFACE TO BE REPAIRABLE IAW SRM 53-00-50-2R-0 REPAIR GENERAL TABLE 201 REPAIR 1<BR>CLEANED AND PREPPED UPPER SURFACE IAW SRM 53-00-50-2R-1 PARAGRAPH 3A;C;E;F<BR>VERIFIED REPAIR MATERIALS AS-- REPAIR PLIES-BMS9-3TYH3 (A10273); RESIN-EPOCAST50A1/9816 (A108753)<BR>NEED OK TO BOND; [02] OK; [03] BONDED REPAIR; CURED 3.5 HOURS AT 150 DEGREES IAW SRM 53-00-50-2R-1 PARAGRAPH 3K;L;M. TAP TEST GOOD. TOOLING AAR30347 DUE 4-29-22; [04] REPAIRED DAMAGE TO UPPER SURFACE FLOOR BOARD IAW SRM 53-00-50-2R-0 REPAIR GENERAL AND SRM 53-00-50-2R-1 REPAIR 1. TAP TEST GOOD; [05] VERIFIED STEPS 3-4