What was found
RH TRANSITION ANGLE 727B-727D HAS CORROSION AROUND MULTIPLE FASTNER HOLES. MARKED.<[01] REMOVE LIGHT SURFACE CORROSION ON RH TRANSITION ANGLE FROM STATION 727B-727D. MATERIAL REMAINING THICKNESS .038. ALL WORK REFERENCE TO SRM 50-00-53-1A-2.;[02] REMOVE LIGHT SURFACE CORROSION ON RH TRANSITION ANGLE FROM STATION 727B-727D. MATERIAL REMAINING THICKNESS .038. ALODINE AND PRIME BLENDED AREA. ALL WORK REFERENCE TO SRM 53-00-53; AMM 51-21-41 AND 51-21-72.;[03] REMOVE LIGHT SURFACE CORROSION ON RH TRANSITION ANGLE FROM STATION 727B-727D. MATERIAL REMAINING THICKNESS .038. ALODINE AND PRIME BLENDED AREA. ALL WORK REFERENCE TO SRM 53-00-53-1A-2; AMM 51-21-41 AND 51-21-72.;[04] VERIFIED REMOVE LIGHT SURFACE CORROSION ON RH TRANSITION ANGLE FROM STATION 727B-727D. MATERIAL REMAINING THICKNESS .038. ALODINE AND PRIME BLENDED AREA. ALL WORK REFERENCE TO SRM 53-00-53-1A-2; AMM 51-21-41 AND 51-21-72.