What was found
FWD WET AREA; GALLEY DOOR ENTRY Z ANGLE HAS AN AREA OF BARE METAL BETWEEN STA 328-344 IN RADIUS.<[01] UPON PREPPING AREA FOR TREATMENT THE AREA WAS DETERMINED TO HAVE CORROSION. CORROSION WILL BE WORKED ON FAULT ID TTG8Q00PV04E;[02] VERIFIED CA#1 UPON PREPPING AREA FOR TREATMENT THE AREA WAS DETERMINED TO HAVE CORROSION. CORROSION WILL BE WORKED ON FAULT ID TTG8Q00PV04E;[03] CORROSION CLEANED ON TASK CARD TTG8Q00PV04E . ALODINE AND PRIMED REWORKED AREA PER SRM 51-20-01.;[04] C/W INSPECTION OF C/A #3