JASC 5753
Service difficulty reports · 31,521
Reports filed under 5753 · Trailing Edge Flaps, newest first.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5753' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE jasc_code = '5753' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR UPS204178Spar · crackedWHILE IN C-CHECK, MAINTENANCE FOUND R/W I/B MIDFLAP LOWER AFT SPAR CHORD CRACKED AT I/B AFT FLAP DRUM ROD CUTOUT. MAINTENANCE REPAIRED IAW SRM 57-50-02, 57-10-1, 51-30-02.SDR UPS204170Support · corrodedWHILE IN FOR C-CHECK, MAINTENANCE FOUND THE O/B MIDFLAP O/B BACK SUPPORT FOR DRUM IS CORRODED. MAINTENANCE REPAIRED PER SRM 51-30-5 AND 51-30-2.SDR UPS204169Rib · crackedWHILE IN FOR C-CHECK, MAINTENANCE FOUND THE LEFT WING I/B MIDFLAP O/B TRACK I/B RIB IS CRACKED. MAINTENANCE INSTALLED NEW RIBS IAW SRM 51-30-2.SDR UPS204158Rib Fitting · crackedWHILE IN FOR C-CHECK, MAINTENANCE FOUND THE R/W I/B MIDFLAP O/B TRACK I/B RIB FITTING WAS CRACKED IN 2 PLACES. MAINTENANCE REMOVED THE CRACKED FITTING AND INSTALLED NEW RIB FITTINGS IAW SRM 51-30-2.SDR UPS204157Fitting · corrodedWHILE IN FOR C-CHECK, MAINTENANCE FOUND CORROSION RUST ON THE FWD ATTACH FITTING FOR THE NR 4 FLAP TRACK. MAINTENANCE REMOVED THE CORRODED FITTING AND REPLACED WITH NEW FITTING IAW MM 27-51-31, SRM 51-30-2 AND MM 27-51-31.SDR MALA954585Doubler · wornDURING SCHEDULED MAINTENANCE IN MSP, THE RIGHT FLAP ROLLER DOUBLER WAS WORN. REPAIRS WERE COMPLETED BY REPLACING THE DOUBLER IAW FAC 57-10-9207 AND ARP 57-20-9024. (M)SDR DL72S953795Spar · crackedDURING SHOP VISIT, FOUND THE NR 2 MIDFLAP AFT SPAR RAIL CRACKED 21 INCHES AND 56 INCHES FROM I/B END OF FLAP. REPAIRED PER M/M57-52-0.SDR 95ZZZX4512Rib · crackedDURING ANNUAL INSPECTION, FOUND SKIN CRACKED ON RT FLAP LEADING EDGE WHERE FLAP ACTUATOR ATTACHES TO FLAP. FOUND LEADING EDGE RIB BROKEN. BROKEN RIB NOT VISIBLE FOR INSPECTION. PROBLEM CAUSES SKIN TO CRACK OUT AT FLAP ACTUATOR ATTACH BRACKET. REPAIR DIFFICSDR 9513211221Vane · delaminatedDURING PERIODIC CHECK, FOUND DELAMINATION IN THE LEFT WING INBOARD FLAP VANE UPPER SURFACE. REPLACED VANE. MFG. P/N NRC6062-519.SDR 9513201221Vane · delaminatedDURING PERIODIC CHECK, FOUND DELAMINATION IN THE LEFT WING OUTBOARD FLAP VANE LOWER SURFACE. REPLACED VANE. MFG. P/N NRC6068-513.SDR 95FDEA01116Spar · corrodedR/W I/B FOREFLAP I/B END POTTING COMPOUND MISSING. REMOVEDUPPER SKIN SURFACE OF FLAP, FOUND L/E SPAR CORRODED. REMOVED CORRODED SPAR AND REPLACED WITH NEW SPAR. LAYED UP SKIN REPAIRS. ALL WORK DONE IAW FEDEX SRM 51-40-6, 51-30-2 AND FEDEX MM 51-20-151, 51-SDR 95FDEA01107Spar · corrodedR/W I/B FOREFLAP I/B END POTTING COMPOUND MISSING. REMOVED UPPER SKIN SURFACE OF FLAP, FOUND L/E SPAR CORRODED. REMOVED CORRODED SPAR AND REPLACED WITH NEW SPAR LAID UP SKIN REPAIRS, ALL WORK DONE IAW FEDEX SRM 51-40-6, 51-30-2 AND FEDEX MM 51-20-151 AND 51-SDR 9512589604Skin · crackedDURING ACCEPTANCE CHECK AND PRIOR TO SERVICE, FOUND A CRACK IN THE RIGHT FLAP NR 2 TRAILING EDGE SEGMENT. REPAIRED PER SRM 51-70-2.SDR CAL950718Struts · brokenBOS - FLT 1246 - TWO TO THREE UNITS OF LEFT WING DOWN WERE REQUIRED TO KEEP WINGS LEVEL AT FLAPS 1, 5, AND 10. MAINTENANCE FOUND THE RT WING CENTER OUTBOARD FLAP TRACK FAIRING STRUTS BROKEN WITH CAM TRACK DAMAGED AND THE PUSHROD FOR AFT FLAP BEARING BROKEN. SDR AALA951436Skin · chafedAFW - FLAP NOSE SKIN IS CHAFED BEYOND SRM LIMITS. BLENDED DYE-CHECKED ALODINED, PRIMED, FILLED WITH BMS 5-28 SEALANT AND PAINTED AREA PER ENGINEERING MRB 767-287. T.S.T. 14,105. CYCLES, 2,184. (X)SDR 95ZZZM593Rib · crackedDURING ROUTINE MAINTENANCE, A CRACK WAS FOUND FOURTH RIB INBOARD 1.5 INCHES UP FROM TRAILING EDGE. REPAIRED WITH PATCH.SDR 95ZZZM479Flap · crackedDURING ROUTINE MAINTENANCE, A .5 INCH CRACK WAS FOUND INBOARD OF ATTACH POINT. REPAIRED WITH PATCH. (M)SDR UPS204106Support Rib · crackedWHILE IN FOR C-CHECK, MAINTENANCE FOUND CRACK SUPPORT RIB IN THE R/W I/B MIDFLAP TRAILING EDGE COVE 52 INCHES FROM THE I/B END. INSTALLED NEW RIB IAW SRM 51-30-5, 51-10-1, 51-30-2.SDR P5CA9500757Canoe Fairing · delaminationDELAMINATION AND PUNCTURE NR 7 CANOE FAIRING. REPAIRED PER BOEING SRM.SDR P5CA9500752Spar · corrodedCORROSION ON RIGHT WING INBOARD MIDFLAP REAR SPAR UPPER T-CHORD, APPROXIMATELY WBL 230. CORROSION REMOVED AND SURFACE REPROTECTED PER BOEING SRM 51-10-01.SDR P5CA9500751Skin · delaminatedDELAMINATION ON RIGHT WING INBOARD MIDFLAP, OUTBOARD UPPER PANEL. REPAIRED PER BOEING SRM 51-40-09.SDR P5CA9500750Le Skin · puncturedPUNCTURE RIGHT WING OUTBOARD FOREFLAP AT OUTBOARD LEADING EDGE. REPAIRED PER BOEING SRM 51-40-09.SDR P5CA9500749Skin · puncturedSMALL PUNCTURE HOLE IN RIGHT WING INBOARD MIDFLAP FORWARD OF NR 5 CANOE FAIRING. REPAIRED PER BOEING SRM 51-40-09.SDR P5CA9500730Fairing · delaminatedDELAMINATION OF NR 8 CANOE FAIRING AT BOTTOM. REPAIRED PER BOEING SRM 51-40-09.SDR P5CA9500728Fairing · puncturedPUNCTURE IN NR 1 TRAILING EDGE FLAP MOVABLE FAIRING. FIBERGLASS REPAIR COMPLETED PER BOEING SRM 51-40-09SDR P5CA9500700Le Skin · gougedRIGHT OUTBOARD FLAP, FOREFLAP OUTBOARD END LEADING EDGE IS GOUGED IN 3 PLACES. REPAIRED PER BOEING SRM 51-40-09.SDR UPS204051Rib · crackWHILE IN FOR C-CHECK, MAINTENANCE FOUND CRACKED SUPPORT RIB ON THE R/W I/B MIDFLAP IN THE TRAILING EDGE COVE 53 INCHES FROM THE O/B END. INSTALLED NEW RIB IAW SRM 51-101 AND 51-30-2.SDR UPS404102Le Skin · crackedWHILE ON GROUND MAINTENANCE FOUND LT WING, INBD MID FLAP LEADING EDGE INBD SECTION HAS A HOLE APPROX 1 INCH DIAMETER AND A CRACK EMANATING FROM IT THAT IS APPROX 10 - 12 INCHES LONG. REPAIRED PER SRM 747-51-40-9.SDR UPS204025Rib · crackedWHILE IN FOR C-CHECK, MAINTENANCE FOUND LT O/B FOREFLAP CENTER LINK TO TRACK ATTACH BOLT IS CHAFING ON MIDFLAP CUTOUT RIB. FOUND CHAFED AREA TO HAVE CRACK REMOVED AND REPLACED RIB PER SRM 51-30-2.SDR DL72S953504Spar · crackedNR 2 MIDFLAP, AFT LOWER SPAR CHORD IS CRACKED 37, 52 INCHES FROM I/B END OF FLAP AND 43 INCHES FROM O/B END OF FLAP. REPAIRED PER M/M 57520 PG 802 AND 807, INSTALLED DOUBLERS. FOUND AT HMV SHOP VISIT.SDR AWXA9500509Flap Track · corrodedPHX - DURING SCHEDULED C-15 INSPECTION,FOUND NR 2 FLAP TRACK CORRODED AT AFT SPAR PARTING SURFACE. REMOVED AND REPLACED FLAP TRACK ASSY PER BMM 27-51-151, PAGE 406. (M)SDR UPS204019Fitting · crackedWHILE IN FOR C-CHECK, MAINT FOUND LT WING INBD MIDFLAP INBD YOKE HOUSING HAS CRACK IN BOTTOM OF GOUGE. REMOVED AND REPLACED FITTING PER SRM 51-30-2, OHM 57-52-111, MM 27-51-22.SDR UPS204018Skin · delaminatedWHILE IN FOR C-CHECK, MAINT FOUND RT WING INBD FOREFLAP HAS DELAM ON UPPER SURFACE. REMOVED DISBONDED SKIN AND DELAMINATION OF PREV REPAIR. FINAL REPAIR PER SRM 51-40-6.SDR UPS204017Skin · delaminatedWHILE IN FOR C-CHECK, MAINT FOUND LT WING INBD FLAP IS DELAMINATING AROUND RUB STRIP INBD END. REMOVED RUB STRIP AND DAMAGED SKIN UNDER RUB STRIP. FINAL INSTALLATION PER SRM 51-40-6, MM 51-51-11.SDR UPS203999Skin · delaminatedWHILE IN FOR C-CHECK, MAINT FOUND RT WING INBD FOREFLAP HAS 1 DELAM ON UPPER SURFACE AT INBD END. REPAIRED PER SRM 51-40-0.SDR 95ZZZM453Fitting · crackedMCI - DURING OP-15 FOUND RIGHT WING RS AFT FLAP CENTER HINGE FITTING MOUNT AREA REAR SPAR WEB, CRACKED .75 INCH IN EYEBROW AT UPPER OUTBOARD HOLE. STOP DRILLED CRACK AND INSTALLED DOUBLER PER SB 57-179 AND DRAWING J060272-502.SDR 95FDEA01075Skin · punctureL/W I/B FOREFLAP HAS A PUNCTURE ON UPPER SURFACE 64 FROM I/B END. L/W I/B FOREFLAP WAS REPAIRED I/W FEDEX SRM 51-40-6.SDR 95FDEA01074Skin · dentedL/W I/B AT FLAP DENTED LWR SURFACE 56 FROM I/B END. L/W I/B AFT FLAP REPAIRED IAW FEDEX SRM 51-40-6.SDR CAL950710Te Panel · delaminatedHOU - INSPECTION FOUND THE LOWER TRAILING EDGE PANEL DELAMINATED JUST OUTBOARD OF NR 1 FLAP HINGE. THE PANEL WAS REPAIRED PER SRM 51-90-0. (M)SDR 95ZZZM478Flap · crackedDURING ROUTINE MAINTENANCE, A CRACK WAS FOUND 10 INCH FROM O/B EDGE 3.5 INCH FROM TRAILING EDGE. REPAIRED WITH PATCH 4 INCH BY 5 INCH. (M)SDR UPS803957Vane · delaminatedWHILE IN DALFORT FOR C-CK, MAINT FOUND LT WING NR 2 FLAP VANE DELAM. REPLACED PER MM 27-51-14.SDR UPS403952T-Chord · crackedWHILE IN AMSTERDAM FOR C-CK, MAINT FOUND RT OUTBD MIDFLAP ASSY UPPER REAR SPAR T-CHORD (P/N G5BCB532-4), IS CRACKED AND HAS LOCAL CORROSION. REPLACED IAW OHM 57-52-55.SDR MALA954565Doubler · wornMSP - DURING A SCHEDULED INSPECTION, MAINTENANCE PERSONNEL FOUND WEAR ON THE LT FLAP WALKING BEAM ROLLER DOUBLER. THEY REPLACED THE DOUBLER WITH A SERVICEABLE DOUBLER IAW FAIRCHILD SRM 57-90-10. (X)SDR MALA954561Doubler · wornMSP - DURING SCHEDULED INSPECTION, MAINTENANCE PERSONNEL FOUND WEAR ON THE RT FLAP WALKING BEAM ROLLER DOUBLER. THEY REPLACED THE DOUBLER WITH A SERVICEABLE DOUBLER IAW FAIRCHILD SRM 57-90-10. (X)SDR UPS 803924Fitting · crackedWHILE IN DALFORT FOR C-CHECK, RT FLAP STA 98 FITTING ON INBD SIDE HAS A 1 INCH CRACK. REPLACED FITTING PER SRM 51-1-20D.SDR CAL950666Fitting · corrodedTHE LEFT INBOARD FLAP TRACK FORWARD SUPPORT FITTING WAS FOUND CORRODED IN THE INBOARD RADIUS FOR THE TRUNNION PIN. THE SUPPORT FITTING WAS REMOVED AND REPLACED IAW MM 27-51-31. (M)SDR DL72L953334Shim · migratedDURING INSPECTION, A LAMINATED SHIM INSTALLED ON THE LEFT WING, INBD T/E FLAP, INBD TRACK WAS FOUND TO HAVE MIGRATED GREATER THAN THE 0.25 LIMIT SPECIFIED PER DAL SI 4-58662-12AD. IN COMPLIANCE WITH AD 90-07-05, THE MIGRATED SHIM WILL BE RELOCATED AND THE ATTSDR ABXA9500664Angle · crackedDURING C - CHECK INSPECTION, FOUND LEFT FLAP ATTACH ANGLE FOR OUTBOARD HINGE CRACKED INSIDE THE FLAP. REPLACED ANGLE IAW DC-9 SRM 51-30-2 AND 51-30-5.SDR ABXA9500663Angle · crackedDURING C - CHECK INSPECTION, FOUND LEFT FLAP ATTACH ANGLE FOR OUTBOARD HINGE CRACKED INSIDE THE FLAP. REPLACED ANGLE IAW DC-9 SRM 51-30-2 AND 51-30-5.SDR 9511732712Skin · delaminatedDURING LINE CHECK, FOUND 4 DELAMINATION IN THE LEFT INBOARD TRAILING EDGE FLAP. REPAIRED PER SRM 51-40-6.
Back to JASC 5753