Boeing 737-4B7
Service difficulty reports · 5,757
Newest first. General aviation reporting is voluntary.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = '7374B7' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = '7374B7' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR USAA051553Frame · crackedSTA400, S9R, MAJOR REPAIR, REMOVED DAMAGE, INSTALL 2 ANGLED DOUBLERS IAW TR 53-10-20C. DEFECT SIZE: .375 IN.SDR USAA051523Bushing · corrodedFOUND CORROSION R4 CLEVIS FWD FACE BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 SPOTS OF CORROSION.SDR USAA051514Bushing · corrodedFOUND CORROSION R2 DUG AFT BUSHING FWD FACE. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051515Bushing · corrodedFOUND CORROSION L1 CLEVIS. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 SPOTS OF CORROSION.SDR USAA051516Bushing · corrodedFOUND CORROSION L4 CLEVIS FWD FACE OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW 55-10-10. DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051517Bushing · corrodedFOUND CORROSION L3 CLEVIS AFT FACE OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051518Bushing · corrodedFOUND CORROSION L3 CLEVIS FWD FACE OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051519Bushing · corrodedFOUND CORROSION, R13 CLEVIS FWD AND AFT FACES OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051520Bushing · corrodedFOUND CORROSION R15 CLEVIS FWD AND AFT FACES. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-1, DEFECT SIZE: .250 DIA SPOTS OF CORROISON.SDR USAA051522Bushing · corrodedFOUND CORROSION R8 LUG FWD AND AFT FACES OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051513Bushing · corrodedFOUND CORROSION L6 CLEVIS AFT FACE. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .250 DIA SPOTS OF CORROSION.SDR USAA051521Bushing · damagedFOUND R6 CLEVIS FWD FACE OF BUSHING. REMOVED DAMAGE, FABRICATED AND INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE:SDR SB05166Battery Pack · dischargedCLT - THE EMERGENCY LIGHTS AT ROWS 14, 16, 18 AND 23 ILLUMINATED BRIEFLY. MAINTENANCE REPLACED THE RIGHT BATTERY PACK. OPERATIONALLY CHECKS OK.SDR USAA051502Frame · crackedFOUND CRACK FS 615 RIGHT SIDE ON INNER CORD ANGLE JUST BELOW CABIN FLOOR. REMOVED DAMAGE, FABRICATED AND INSTALLED FILLERS AND DOUBLERS IAW TR 53062-01, DEFECT SIZE: 1.5".SDR USAA051510Mount · corrodedFOUND CORROSION RT HORIZ STAB R1 LUG FWD FACE AND BORE. SPOT FACED FWD FACE OF LUG, INSTALLED NEW BUSHINGS IAW SRM 55-10-10 SRM 52-10-10, DEFECT SIZE: .375".SDR USAA051494Frame · crackedFOUND FRAME CRACKED STA 827 S9L. REMOVED DAMAGE, INSTALL ANGLED DOUBLER AND TRIPLER IAW TYP REP 53-10-20C, DEFECT SIZE: .500".SDR USAA051497Clevis · corrodedFOUND RT HORIZ STAB R12 CLEVIS BOTH FACES. SPOT FACE BOTH FACES, INSTALL NEW BUSHING AND SHIMS IAW SRM 55-10-10, DEFECT SIZE: .325".SDR USAA051498Clevis · corrodedFOUND FWD AND AFT FACE OF R3 CLEVIS. SPOT FACED BOTH FACES INSTALLED NEW BUSHING IAW SRM 55-10-10, DEFECT SIZE: .375.SDR USAA051499Clevis · corrodedFOUND CORROSION RIGHT STAB CENTER SECTION CLEVIS NR 9 BOTH FACES. SPOT FACE BOTH FAVES, REPLACE BUSHING IAW SRM 55-10-10, DEFECT SIZE: .375".SDR USAA051492Pressure Panel · crackedFOUND CRACK FUSELAGE STATION 664 LBL 30. REMOVED DAMAGED AREA, FABRICATED AND INSTALLED A NEW STIFFENER ANGLE AND SHIMS IAW TR 53-60-04, DEFECT SIZE: 2.3"SDR USAA051501Angle · corrodedFOUND CORROSION FWD ENTRY DOOR Z ANGLE STA 306-346. REMOVED DAMAGED Z ANGLE AND INSTALLED A NEW Z ANGLE IAW 53-10-15 FIG 101, DEFECT SIZE: 38".SDR USAA051505Angle · damagedFOUND GROOVE RIGHT AFT DOOR SILL FUSELAGE STATION 967. REMOVED AND REPLACED ANGLE IAW SRM 51-10-02 DEFECT SIZE: 11"SDR USAA051506Intercostal · crackedFOUND CRACK STA 294.5 S7L. REPLACED DAMAGED PART WITH NEW PART IAW SRM 51-10-02 DWG 65-17684, DEFECT SIZE: .250".SDR USAA051508Clevis · corrodedFOUND HORIZ STAB CENTER SECTION R7 CLEVIS CORRODED. REMOVED BUSHING REAMED BORE SPOT FACED BOTH FACES INSTALLED NEW BUSHINGS AND SHIMS IAW SRM 55-10-10, DEFECT SIZE: .375".SDR USAA051509Attach Fitting · corrodedFOUND CORROSION RT HORIZ STAB, FWD FACE OF R5 LUG. SPOT FACED LUG AND INSTALLED NEW BUSHINGS IAW SRM 55-10-10 SRM 52-10-10, DEFECT SIZE: .375".SDR USAA051500Frame · crackedFOUND CRACK STA 480 S9R. REMOVED DAMAGE, INSTALLED TWO REPAIR ANGLES IAW 53-10-20C, DEFECT SIZE: 1.000".SDR USAA051490Angle · corrodedFOUND FWD GALLEY AREA CORRODED STA 277-360RBL. MAJOR REPAIR, NEW Z ANGLE PREVIOUSLY INSTALLED IAW BOEING DRWG 65-45834, DEFECT SIZE: .250.SDR USAA051493Splice · crackedFOUND CRACK BS908 AT STRINGER 4. DEFECTIVE PART REPLACED WITH IDENTICAL PART IAW SRM 51-10-02, DEFECT SIZE: .500".SDR USAA051484Frame · crackedFOUND FRAME DAMAGED STA 727E, S8R-S9R. REMOVED DAMAGE INSTALLED ANGLED DOUBLER AND ANGLED TRIPLER IAW TYP REP 53-10-20, DEFECT SIZE: FUSELAGE FRAME CRACKED AT RT PSU RAIL ATTACH BRACKET.SDR USAA051488Frame · crackedFOUND FRAME CRACKED STA 787, S 9L. CUT OUT DAMAGED AREA AND INSTALLED REPAIR DOUBLERS IAW TR 53-10-2C, DEFECT SIZE: 1" CRACK.SDR USAA051487Frame · crackedFOUND FRAME BS 747 BETWEEN S8-S9R AT PSU ATTACH BRACKET. CUT OUT DAMAGE AND INSTALLED REPAIR DOUBLERS IAW TR 53-10-2C, DEFECT SIZE: 1" CRACK.SDR USAA051485Attach Angle · crackedFOUND CRACK RT PYLON UPPER IB AFT AREA, NAC STA 314.24. REMOVED AND REPLACED ATTACH ANGLE IAW SRM 51040-02, DEFECT SIZE: .250" CRACK.SDR USAA051476Frame · crackedFOUND FRAME CRACKED BS 727D. REMOVED DAMAGE AND INSTALLED REPAIR DOUBLER IAW TR 53-10-20C, DEFECT SIZE: FUSELAGE FRAME CRACKED AT LT PSU RAIL ATTACH BRACKET, CRACK MEASURES .65 INCHES.SDR USAA051477Floorbeam · corrodedFOUND FLOORBEAM UPPER T CAP CORRODED, BS 328; LBL 60. FAB`D AND INSTALLED NEW T-CAP SECT REPAIR SPLICE IAW 53-10-51, FIG 201, DEFECT SIZE: 1/2" BY 1/2" CORRODED AREAS AROUND CLIP NUT HOLES.SDR USAA051478Intercostal · corrodedFOUND INTERCOSTAL CORRODED AT STA 312-328, RBL 12. REMOVED AND REPLACED INTERCOSTAL IAW SRM 51-10-02, DEFECT SIZE: .50" AREAS OF CORROSION AT EACH FASTENER HOLE.SDR USAA051479Intercostal · corrodedFOUND CORROSION STA 328-344, LBL9. REMOVED AND REPLACED IAW SRM 51-10-02 DEFECT SIZE: .5 INCH AREAS OF CORROSION ON THE INTERCOSTAL 16 INCHES IN LENGTH.SDR USAA051480Intercostal · corrodedFOUND CORROSION STA 312-328, LBL9. REMOVE AND REPLACE INTERCOSTAL IAW SRM 51-10-02, DEFECT SIZE: .5" AREAS OF CORROSION ON THE INTERCOSTAL 16" IN LENGTH.SDR USAA051482Intercostal · corrodedFOUND INTERCOSTAL CORRODED STA 947-967, LBL. REMOVED AND REPLACED WITH NEW PART IAW SRM 51-10-02, DEFECT SIZE: .350" AREA OF CORROSION AT FASTENER HOLE, 20 INCHES IN LENGTH.SDR USAA051481Fitting · crackedRT MLG FWD TRUNNION TO AFT SPAR FITTING 6:00 POSITION AT HOLE B. INSTALLED TWO NEW FASTENERS IAW TR 57-10-13 REV A DEFECT SIZE: RT MLG BEAM AFT SUPPORT FITTING CRACKED AT 6:00 IN HOLE B, CRACK IS .5" LONG.SDR USAA051471Angle · corrodedAFT ENTRY DOORWAY Z-ANGLE CORRODED. MAJOR REPAIR, REPLACED WITH IDENTICAL PART, IAW SRM 51-10-02 STEP 8. DEFECT SIZE: .250 X .250 INCH TO 1 X 2 INCH.SDR USAA051472Angle · corrodedZ-ANGLE AT FWD SERVICE DOOR FROM STA 294 TO 330 CORRODED. MAJOR REPAIR, REMOVED AND REPLACED WITH NEW Z-ANGLE IAW SRM 51-10-02 STEP 8. DEFECT SIZE: .250 X .250 INCH TO 1 X 2 INCH.SDR USAA051470Support Angle · corrodedFWD SERVICE DOOR SCUFF PLATE SUPPORT ANGLE CORRODED. REPLACED WITH IDENTICAL PART, REMOVED CORRODED ANGLE & REINSTALLED NEW ANGLE IAW SRM 51-10-2. DEFECT SIZE: APPROX .5 X 24 INCH CORRODED AREA.SDR USAA051462Crease Beam · corrodedSTA 615 TO 639 LEFT CORRODED. MAJOR REPAIR, REMOVED CORROSION AND TREATED IAW SRM 53-60-13, DEFECT SIZE: 2 INCHES.SDR USAA051467Floorbeam · corrodedSTA 986.5 LBL 8 TO EXTREME RT END. MAJOR REPAIR, REMOVED DAMAGED T-CAP, INSTALLED NEW REPAIRED PART IAW SRM 53-60-01 REV A. DEFECT SIZE: 1 INCH.SDR USAA051466Stringer Clip · crackedSTA 727G, S4R CRACKED. MAJOR REPAIR, REPLACED TIE CLIP IAW SRM 51-10-02, DEFECT SIZE: .5.SDR USAA051465Stringer Clip · crackedSTA 727E S4L. MAJOR REPAIR, REPLACED TIE CLIP IAW SRM 51-10-02, DEFECT SIZE: .6.SDR USAA051454Floorbeam · corrodedUPPER FLANGE STA 986.5 - LBL 30 CORRODED. MAJOR REPAIR, INSTALLED FLOORBEAM UPPER CHORD REPAIR IAW SRM 53-60-51 FIG 201, DEFECT SIZE: .250.SDR USAA051461Stringer Clip · crackedSTA 727E, S4L CRACKED. MAJOR REPAIR, REPLACED TIE CLIP IAW SRM 51-10-02.SDR USAA051460Stringer Clip · crackedSTA 727G S4R CRACKED. MAJOR REPAIR, REPLACED TIE CLIP IAW SRM 51-10-02.SDR USAA051459Skate Angle · wornRT SIDE VERTICAL STAB AT FIN WL 0.0 HAS WEAR. MAJOR REPAIR, FABRICATED AND INSTALLED REPAIR PART IAW TR 53-20-05A, DEFECT SIZE: 1 INCH.
Back to Boeing 737-4B7