Boeing 737-8H4
Service difficulty reports · 24,314
Newest first. General aviation reporting is voluntary.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = '7378H4' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = '7378H4' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR SWAA2023071874658Scuff Plate · crackedAFT CARGO BAY AFT CORNER SCUFF PLATE IS CRACKED<[01] WELDED CRACK ON AFT CARGO BAY AFT CORNER SCUFF PLATE USING ER4043 ALUMINUM FILLER ROD LOT NUMBER 1131216 PER SRM 53-60-15-2R-1 PARAGRAPH 4. B. (2) AND (4). REPAIR AREA STILL REQUIRES A DYE PENETRANT INSPECTISDR SWAA2023070675210Girt Bar · missingWHITE PLASTIC SERVICE MISSING FROM FWD SERVICE GRIT BAR<[01] REMOVED AND REPLACED FWD SERVICE DOOR GIRT BAR OPS CK NORMAL IAW AMM 25-00-00SDR SWAA2023070674899Plate · looseAFT GALLEY DOOR CENTER CAM PLATE IS LOOSE<[01] ADJUST CAM PLATE PER AMM 52-41-11.SDR SWAA2023081681722Bracket · crackedLEFT WING FRONT SPAR STATION IFFS 150 ANTI ICE DUCT SUPPORT BRACKET IS CRACKED VIEW WITH LEADING EDGE FLAP EXTENDED<[01] REMOVED AND REPLACED SUPPORT BRACKET AT L/W FRONT SPAR STATION IFFS 150 REF B-737-800 SRM 51-40-02-0G-0; SRM 51-40-04-0G-0 TOOL USED ; TORQSDR SWAA2023080474793Support Angle · corrodedAFT CARGO BELT FRAME HAS CORROSION IN AND AROUND N/P HOLE BS727I RBL23.<[01] REMOVED CORROSION FROM AFT CARGO BELT FRAME (PANEL SUPPORT ANGLE) IN AD AND AROUND N/P HOLE BS 727I RBL 23 PER AMM 51-00-53/201. MECHANICALLY MEASURED ANGLE TO BE 0.063? ORIGINAL THICSDR SWAA2023080474797Angle · corrodedAFT CARGO LT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727F-727G.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727F- 727G. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.007?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.03SDR SWAA2023080474798Angle · corrodedAFT CARGO LT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727G-727H.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727G- 727H. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.005?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.03SDR SWAA2023080474799Angle · corrodedAFT CARGO LT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727H-727I.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727H-727I. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.008?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.032SDR SWAA2023080474800Angle · corrodedAFT CARGO LT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727I-727J.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727I-727J. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.007?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.033SDR SWAA2023080474802Angle · corrodedAFT CARGO TRANSITION ANGLE LBL 22' STA.727J TO STA.747. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727J-747. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.007?; MAX ALLOWED IS 0.004?; REMAININGSDR SWAA2023080474801Angle · corrodedAFT CARGO LT. TRANSITION ANGLE HAS CORROSION AROUND FASTENER BS727F.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 727F. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.005?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.035?. FOUND TO BE OUTSDR SWAA2023080474806Angle · corrodedAFT CARGO TRANSITION ANGLE LBL 22' STA.747 TO STA.767. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 747-767. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.007?; MAX ALLOWED IS 0.004?; REMAINING TSDR SWAA2023080474808Angle · corrodedAFT CARGO TRANSITION ANGLE LBL 22' STA.767 TO STA.787. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 22 STA 767-787. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.008?; MAX ALLOWED IS 0.004?; REMAINING TSDR SWAA2023080474809Angle · corrodedAFT CARGO TRANSITION ANGLE RBL 22' STA.767 TO STA.787. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE RBL 22 STA 767F TO STA. 787 ORIGINAL THICKNESS IS 0.050?; MATERIAL LOSS IS 0.006?; MAX ALLOWED IS 0.005?; REMSDR SWAA2023080474784Angle · corrodedAFT CARGO TRANSITION ANGLE LBL 23' STA.787. HAS AREAS OF CORROSION AROUND FASTENER HOLE.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 23 STA 787. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.008?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.03SDR SWAA2023080474810Angle · corrodedAFT CARGO TRANSITION ANGLE LBL 23' STA.807 HAS AREAS OF CORROSION AROUND FASTENER HOLE.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE LBL 23 STA 807. ORIGINAL THICKNESS IS 0.040?; MATERIAL LOSS IS 0.007?; MAX ALLOWED IS 0.004?; REMAINING THICKNESS IS 0.033SDR SWAA2023080474785Angle · corrodedAFT CARGO TRANSITION ANGLE RBL 22' STA.847 TO STA.867. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED CORROSION AFT CARGO TRANSITION ANGLE RBL 22 STA 847F TO STA. 867 ORIGINAL THICKNESS IS 0.050?; MATERIAL LOSS IS 0.003?; MAX ALLOWED IS 0.005?; REMSDR SWAA2023080274814Angle · crackedAFT CARGO LAV TANK WALL SUPPORT VERTICAL ANGLE CRACKED STA. 867 LBL16' WL 166'<[01] REMOVED CRACKED ANGLE PER SRM 51-40-02;[02] REMOVED AND REPLACED AFT CARGO LAV TANK WALL SUPPORT VERTICAL ANGLE STA. 867 LBL16' WL 166' PER SRM 51-40-02;[03] INSPECTION C/W REMSDR SWAA2023080274792Floor Splice · corrodedAFT CARGO FLOOR SPLICE HAS PRIMER MISSING AND CORROSION IN AND AROUND N/P HOLES BS727D+6.<[01] RECEIVED NEW FLOOR SPLICE. SPLICE WILL BE INSTALLED ON ROUTINE TASK CARD TTG8Q00L8CXJ;[02] VERIFIED NEW SPLICE PROCUREMENT AND TO BE INSTALLED ON CARD TTG8Q00L8CXJ. SDR SWAA2023080274781Floor Splice · corrodedAFT CARGO FLOOR SPLICE HAS PRIMER MISSING AND CORROSION IN AND AROUND N/P HOLES BS727I+5.<[01] RECEIVED NEW FLOOR SPLICE. SPLICE WILL BE INSTALLED ON ROUTINE TASK CARD TTG8Q00L8CXQ;[02] VERIFIED NEW SPLICE PROCUREMENT AND TO BE INSTALLED ON CARD # TTG8Q00L8CXQSDR SWAA2023080174084Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 430<[01] REMOVED CORROSION AT STA. 430 L/H TRANSLON ANGLE MATERIAL REMOVED .006 FOUND OUT OF LIMITS PER SRM 53-00-53-1A-1;[02] C/W INSPECTION;[03] COMPLIED WITH INSPECTION OF THE REPLACED TRANSITION ANGLE FSDR SWAA2023080174085Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 450<[01] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .005 ; FOUND TO BE OUT LIMITS PER SRM. 53-00-53-1A-1;[02] REPLACED TRANSITION ANGLE FROM STATION 420 +7 TO 500D +10 ON NON ROUTINE TTG8Q00LZZM2;[SDR SWAA2023080174086Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 500+5<[01] REMOVED CORROSION PER SRM.51-10-02 ; MATERIAL REMOVED .008 FOUND TO BE OUT OF LIMITS PER SRM. 53-00-53-1A-1;[02] REPLACED TRANSITION ANGLE FROM STATION 420 +7 TO 500D +10 ON NON ROUTINE TTG8Q00LZSDR SWAA2023080174087Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 460-480<[01] REMOVED CORROSION 51-10-02 MATERIAL REMOVED .006 FOUND TO BE OUT OF LIMITS PER SRM. 53-00-53-1A1;[02] REPLACED TRANSITION ANGLE FROM STATION 420 +7 TO 500D +10 ON NON ROUTINE TTG8Q00LZZM2;[03] SDR SWAA2023080174088Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 500A+15<[01] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .003 ; FOUND TO BE WITHIN LIMITS PER SRM. 53-00-53-1A-1;[02] REPLACED TRANSITION ANGLE FROM STATION 420 +7 TO 500D +10 ON NON ROUTINE TTG8Q00SDR SWAA2023080174089Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 500C-500D<[01] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .006 ; FOUND TO BE OUT LIMITS PER SRM. 53-00-53-1A-1;[02] REMOVED SECTION OUT LIMITS L/H TRANSITION ANGLE FROM STA. 430+8 ; TO STA.500D+10 SDR SWAA2023080174090Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 500D-500E<[01] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .006 ; FOUND TO BE OUT LIMITS PER SRM. 53-00-53-1A-1;[02] TREAT AND PRIMED AREA PER SRM 51-20-01;[03] REJECT: DAMAGE FOUND TO BE OUT OF LIMSDR SWAA2023080174091Angle · corrodedFWD CARGO COMPT LH TRANSITION ANGLE HAS CORROSION STA 500E-500F<[01] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .003 ; FOUND TO BE OUT LIMITS PER SRM. 53-00-53-1A-1;[02] REMOVED CORROSION PER SRM.51-10-02 MATERIAL REMOVED .003 ; FOUND TO BE WITHIN LIMSDR SWAA2023080174794Scuff Plate · corrodedAFT CARGO DOOR THRESHOLD SCUFF PLATE WEB HAS AREAS OF LIGHT CORROSION AND BARE METAL<[01] REMOVED AFT CARGO DOOR THRESHOLD SCUFF PLATE WEB IAW SRM 51-40-02;[02] LOCATED; DRILLED; AND COUNTERSUNK NEW AFT CARGO DOOR SCUFF PLATE IAW SRM 51-40-05 AND SRM 51-40-08.SDR SWAA2023080174795Angle · corrodedAFT CARGO RT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727H-727I.<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727H-727I PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .005 AND REMAINING THICKNESSSDR SWAA2023080174796Angle · corrodedAFT CARGO RT. TRANSITION ANGLE HAS CORROSION IN AND AROUND N/P HOLES BS727I-727J.<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727H-727I PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .006 AND REMAINING THICKNESSSDR SWAA2023080174783Angle · corrodedAFT CARGO TRANSITION ANGLE RBL 22' STA.727J TO STA.747. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727H-727I PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .007 ANDSDR SWAA2023080174804Angle · corrodedAFT CARGO RT. TRANSITION ANGLE HAS CORROSION AROUND FASTENER HOLE BS727E<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727E PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .005 AND REMAINING THICKNESS .035 PER SRM SDR SWAA2023080174805Angle · corrodedAFT CARGO RT. TRANSITION ANGLE HAS CORROSION AROUND FASTENER HOLE BS727F<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727F PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .002 AND REMAINING THICKNESS .038 PER SRM SDR SWAA2023080174807Angle · corrodedAFT CARGO TRANSITION ANGLE RBL 22' STA.747 TO STA.767. HAS AREAS OF CORROSION AROUND FASTENER HOLES.<[01] REMOVED LIGHT SURFACE CORROSION AFT CARGO R/H TRANSITION ANGLE FROM STA. 727H-727I PER SRM 51-10-02; FOUND TO BE OUT OF LIMITS. MATERIAL REMOVED .004 AND SDR SWAA2023080174540Floor Support · crackedPASSENGER CABIN STA 540 RBL 2 FLOOR SUPPORT HAS A CRACK<[01] REMOVED AND REPLACED PANEL BREAK PER SRM 51-40-02.;[02] RII: C/W INSPECTION FOR R&R OF PANEL BREAK PER SRM 51-40-02.SDR SWAA2023080174542Floor Support · crackedPASSENGER CABIN STA 540 LBL 2 FLOOR SUPPORT HAS A CRACK.<[01] REMOVED AND REPLACED PANEL BREAK PER SRM 51-40-02.;[02] RII: C/W INSPECTION FOR R&R OF PANEL BREAK PER SRM 51-40-02.SDR SWAA2023071174507Battery Pack · inoperativeSEVERAL EXTERIOR AND INTERIOR EMERGENCY LIGHTS INOPERATIVE.<[01] PERFORMED T/S AS PER WDM 33-51-14 AND FOUND DEFECTIVE BATTERY PACKS AT POSITIONS M1675; M2816; M2335; AND M1676. REPLACED EMERGENCY LICHTS BATTERY PACKS POSITIONS M1675; M2816; M2335; AND M1676. SDR SWAA2023070674196Megaphone · inoperativeFWD MEGAPHONE BROKEN AND INOP<[01] REMOVED AND REPLACED MEGAPHONE PER AMM 25-64-00.SDR SWAA2023070674257Battery Pack · inoperativeLH SLIDE EMERGENCY LIGHT INOP<[01] REF TTG8Q00M01A4 FOR CORRECTIVE ACTION. R&R LH BATTERY PACKS, AND PACK CHARGER AT STA 727C AND STA 565 PER AMM 33-51-06. OP TEST OF EMERGENCY LIGHTS OK.SDR SWAA2023070675462Charger · inoperativeAFT LH EMERGENCY OVERWING EXIT EMERGENCY LIGHT INOP<[01] R&R LH BATTERY PACKS; AND PACK CHARGER AT STA 727C AND STA 565 PER AMM 33-51-06. OP TEST OF EMERGENCY LIGHTS OK.SDR SWAA2023070675822Charger · inoperativeLH SLIDE EMERGENCY LIGHT INOP<[01] REF TTG8Q00M01A4 FOR CORRECTIVE ACTION. R&R LH BATTERY PACKS, AND PACK CHARGER AT STA 727C AND STA 565 PER AMM 33-51-06. OP TEST OF EMERGENCY LIGHTS OK.SDR SWAA2023070675165Battery · inoperativeFLASHLIGHT IN AFT GALLEY FO SIDE DOES NOT TEST.<[01] R&R AFT FO OUTBOARD FLASHLIGHT BATTERY PER AMM 25-64-00. OPS CHECK GOOD.SDR SWAA2023070674258Battery Pack · inoperativeAFT LH EMERGENCY OVERWING EXIT EMERGENCY LIGHT INOP<[01] R&R LH BATTERY PACKS; AND PACK CHARGER AT STA 727C AND STA 565 PER AMM 33-51-06. OP TEST OF EMERGENCY LIGHTS OK.SDR SWAA2023080274065Angle · corrodedFWD GALLEY DOOR CUTOUT LOWER 'L' ANGLE ATTACHED TO Z ANGLE HAS CORROSION 5EA FASTENER HOLES.(MARKED)<[01] REMOVED CORROSION IAW SRM 51-10-02. DAMAGE REMOVAL APPROX .015' OUT OF LIMITS PER SRM 53-10-15-1A-2.;[02] LOCATED/DRILLED FASTENER HOLES IN REPLACEMENT ANSDR SWAA2023080174082Web · cracked#2 ENGINE PYLON STRUT FAIRING AFT WEB CRACKED (MARKED)<[01] REMOVED #2 ENGINE NOZZLE PER AMM 78-11-01;[02] LOCATED; DRILLED; AND COUNTERSUNK NEW TRAILING EDGE SECTION PER SRM 51-40-05 AND SRM 51-40-08.;[03] OK TO INSTALL.;[04] INSTALLED NEW SERVICEABLE #2 PYLOSDR SWAA2023073174200Strap · corrodedCORROSION FOUND AT STA.947 LBL25 UPPER AFT FLANGE AT FLOOR BEAM<[01] REMOVED DAMAGE PER SRM 51-10-02. FOUND TO BE OUT OF LIMITS PER SRM 53-70-51-1A-1.;[02] ADDED TOOLS.;[03] VERIFIED 1. WILSON WHITT (TECHNICIAN); 02-JUL-2023 17:27 UTC<BR>REMOVED DAMAGE PER SRMSDR SWAA2023073174201Strap · corrodedIN THE AFT CABIN WET AREA THERE IS EVIDENCE OF CORROSION ON TOP OF THE FLOOR BEAM AT STATION 947; LBL 16.<[01] REMOVED DAMAGE PER SRM 51-10-02. FOUND TO BE OUT OF LIMITS PER SRM 53-70-51-1A-1.;[02] ADDED TOOLS;[03] VERIFIED 1. WILSON WHITT (TECHNICIAN); 02-JULSDR SWAA2023071173781Structure · elongatedFWD CARGO FWD 2 L/H CAP STRIPS HAVE ELONGATED HOLES.<[01] REMOVED AND REPLACED FWD CARGO L/H CAP STRIPS PER AMM 25-52-10.SDR SWAA2023071173783Battery Pack · inoperativeEMERGENCY EXIT LIGHTS POWER SUPPLY M1694(BS565;LBL68) FAILS CAPACITY CHECK.<[01] REMOVED AND REPLACED BATTERY PACK FOR EMERGENCY EXIT LIGHTS POWER SUPPLY M1694 WITH NEW FROM STOCK IAW AMM 33-51-06. OPS CHECK GOOD.;[02] VERIFIED WORK IN C/A #1
Back to Boeing 737-8H4