What was found
AFT CARGO COMPARTMENT FLOOR SUPPORT ANGLE CORRODED AT SPLICE LWR SURFACE AT STA 1445, LBL 3. AFT CARGO FLOOR SUPPORT SPLICE AT STA 1445, LBL 2.9 REMOVED AND REPLACED IAW SRM 51-40-02 REV 98. CORROSION REMOVED IAW SRM 51-10-02 REV 98. ORIGINAL THICKNESS 0.071", MATERIAL REMOVED 0.016", MATERIAL REMAINED 0.055" FOUND EXCEED LIMIT SRM 53-00-53 FIG 101 REV 98. THIS REPAIR IS CLASSIFIED AS MINOR GMM 6-2-100 CRITERIA.