Par 1-36 Page 1-80 Splicing under minor fittings such as drag wire, antidrag wire, or compression strut fittings is acceptable under the following conditions:
The reinforcement plates of the splice should not interfere with the proper attachment or alignment of the fittings. Do not alter the locations of pulley support brackets, bellcrank support brackets, or control surface support brackets. Plates are to be tapered off, as depicted in figure 1-2.
The reinforcement plate may overlap drag wire, antidrag wire, or compression strut fittings, if the reinforcement plates are on the rear face of the rear spar or the front face of the front spar. In such cases, it will be necessary to install slightly longer bolts. The front face reinforcement plate shoul d not overlap drag strut fittings, except when it does not require sufficient shortening of compression struts or changes in dragtruss geometry, to prevent adjustment for proper rigging. Even though take up is sufficient, it may be necessary to change the angles on the fittings.
(Acceptable methods for splic ing the various types of spars are shown in figure 1-4 through figure 1-9.)
Reinforcement plates must be used as indicated on all scarf repairs to spars and the slopes of scarves shown are minimum slopes.
SPAR REPLACEMENT. Replacement of spars is a major repair. Spars may be replaced by new parts made by the manufacturer or the holder of a Parts Manufacturer Approval (PMA) for that part.
Owner-produced spars may be installed providing they are made from a manufacturer-approved drawing. Also, a spar may be made by reference to an existing spar providing sufficient evidence is presented to verify that the existing spar is an original part, and that all materials and dimensions can be determined. The dimensions and type of wood used are critical to the structural strength of the aircraft. Care should be taken that any replacement spars accurately match the manufacturer’s original design.
SPLICING OF BOX SPAR WEBS. Always splice and reinforce plywood webs with the same type of plywood as found on the original part. Do not use solid wood to replace plywood webs. Plywood is stronger in shear than solid wood of the same thickness due to the grain direction of the individual plies. The face-grain of plywood replacement webs and reinforcement plates must be in the same direction as the original member to ensure that the new web will have the required strength. (The method of splicing plywood webs is shown in figure 1-9.)
REPLACING SOLID-TYPE SPARS WITH LAMINATED-TYPE SPARS. Solid spars may be replaced with laminated spars or vice versa, provided the material is of the same high quality.
External reinforcements (plywood or solid) must always be replaced as on the original member.
SPAR LONGITUDINAL CRACKS AND LOCAL DAMAGE. Cracked spars (except box spars) may be repaired by bonding plates of spruce or plywood of sufficient thickness to develop the longitudinal shear on both sides of the spar. Extend the plates well beyond the termination of the cracks, as shown in figure 1-10. A method of repairing small local damage to either the top or bottom side of a spar is also shown in figure 1-10.
Longitudinal Cracking of Wood Wing Spars of Aircraft Operating in Arid Regions. Aircraft having wood spars and operating in arid regions may develop longitudinal spar cracks in the vicinity of the plywood reinforcement plates. Th ese cracks result from the tendency of the spar to shrink when drying takes place.
Plywood resists this tendency to
Par 1-44 Page 1-81
Reinforcement plates to be spruce or plywood and should be bonded only, with the ends feathered off at 5:1 slope as depicted in Figure 1-2.
Solid spars may be replaced with laminated spars or vice versa, provided the material is of the same high quality.
FIGURE 1-5. Method of splicing solid or laminated rectangular spars.
shrink and causes the basic spar stock to split (see paragraph 1-2c). Cracks start under the plywood plates, usually (but not necessarily) at a bolt hole or cutout, and usually spread in each direction until they extend a short distance beyond the ends of the plates where the resistance to spar shrinkage disappears. Cracks have also been found in the butt end of spars. Other factors, which have been found conducive to the formation of cracks are poor protective finishes, large cutouts, and metal fittings that utilize two lines of large diameter bolts.
Repairing Cracks Versus Installing a New Spar. The presence of cracks does not n ecessarily mean that the spar must be discarded. If the crack is not too long or too close to either edge and can be reinforced properly, it will probably be more economical and satisfactory to perform repair rather than install a new spar or section. However, a generally acceptable procedure suitable for all airplane models is not available. Because of the possibility of strength deficiencies contact the manufacturer. In absence of the manufacturer, the FAA should be contacted for approval before making repairs not in accordance with the manufacturer-approved instructions or the recommendations of this advisory circular. Longitudinal cracking or the recurrence of cracking can be minimized by ensuring that the moisture content of the solid wood portion is within the proper range before bonding . In arid desert areas, during bonding the moisture content should be in the range of 6-8 percent before bonding, but in other areas 10-12 percent is satisfactory. If solid or plywood repair stock is procured from another climatic region, it should be allowed to season,
Par 1-44 Page 1-82
If splice is made where routing is feathered to full width of spar, tapered plates (conforming to the contour of the routing) should be added first;
otherwise, the splice is the same as shown.
Reinforcement plates may be of plywood, the same material as the spar, or material of equal or higher quality; and should be bonded only with ends feathered out with a 5:1 slope.
FIGURE 1-6. Method of splicing solid “I” spars.
in the same storage area as th e part to be repaired, for no less than 2 weeks.
Preventing Cracks. An important step in the prevention of longitudinal cracking, particularly in spar butts, is to ensure that the wood is thoroughly sealed with a penetrating and highly moisture-resistant finish.
Application of a thin, slow-curing epoxy adhesive or sealer can be very effectiv e in slowing or preventing moisture changes in spar butts.
ELONGATED HOLES IN SPARS. In cases of elongated bolt holes in a spar, or cracks in the vicinity of bolt holes, splice in a new section of spar, or replace the spar entirely. If hole elongation or cracking is minimal and the bolt holes are for noncritical fittings, repair (rather than replacement) may be feasible. Obtain approval for any such repair from the manufacturer or a representative of the FAA. In many cases, it has been found advantageous to laminate the new section of the spar, particularly if the spar butts are being replaced.
RIB REPAIRS. Ribs may be replaced by new parts made by the manufacturer or the holder of a PMA for that part. Owner-produced ribs may be installed providing they are made from a manufacturer-approved drawing or by reference to an existing original rib. A rib may be made by reference to an existing rib providing sufficient evidence is presented to verify that the existing rib is an original part and that all materials and dimensions can be determined. The contour of the rib is important to the safe flying qualities of the aircraft, and care should be taken that any replacement ribs accurately match the manufacturer’s original design.
Par 1-46 Page 1-83
Ends of reinforcement plates
should be feathered out Section A-A with a 5:1 slope.
FIGURE 1-7. Repairs to built-up “I” spar.
Rib Repair Methods. Acceptable methods of repairing damaged ribs are shown in figure 1-11. Wood ribs should not be nailed to wood spars by driving nails through the rib cap strips, as this weakens the rib materially. The attachment should be by means of adhesive with cement coated, barbed, or spiraled nails driven through the vertical rib members on each face of the spar.
Compression Rib Repair. Acceptable methods of repairing damaged compression ribs are shown in figure 1-12.
Figure 1-12(A) illustrates the repair of a compression rib of the “I” section type; i.e., wide, shallow cap strips, and a center plywood web with a rectangular compression member on each side of the web. The rib is assumed to be cracked through the cap strips, web member, and compression member in the illustration. Cut the compression member as shown in figure 1-12(D). Cut and replace the aft portion of the cap strips, and reinforce as shown in figure 1-11. The plywood side plates are bonded on, as indicated in figure 1-12(A). These plates are added to reinforce the damaged web.
Figure 1-12(B) illustrates a compression rib of the type that is basically a standard rib with rectangular compression members added to one side and plywood web to the other side. The method used in this repair is essentially the same as
Par 1-46 Page 1-84 in figure 1-12(A) except that the plywood reinforcement plate,
A, B, C, D = ORIGINAL DIMENSIONS
FIGURE 1-8. Method of splicing box spar flanges (plate method).
shown in section B-B, is continued the full distance between spars.
Figure 1-12(C) illustrates a compression rib of the “I” type with a rectangular vertical member on each side of the web. The method of repair is essentially the same as in figure 1-12(A) except the plywood reinforcement plates on each side, shown as striped blocks in section C-C, are continued the full distance between spars.
PLYWOOD SKIN REPAIR. Make extensive repairs to damaged stressed skin plywood structures in accordance with specific recommendations from the aircraft manufacturer. It is recommended that repairs be made by replacing the entire panel, from one structural member to the next, if damage is very extensive. When damaged plywood skin is repaired, carefully inspect the adjacent internal structure for possible hidden damage. Repair any defective frame members prior to making skin repairs.
DETERMINATION OF SINGLE OR DOUBLE CURVATURE. Much of the outside surface of plywood aircraft is curved. On such areas, plywood used for repairs to the skin must be similarly curved.
Curved skins are either of single curvature or of double (compound) curvature. A simple test to determine which type of curvature exists may be made by laying a sheet of heavy paper on the surface in question. If the sheet can be made to conform to the surface without wrinkling, the surface is either flat or single curvature. If the sheet cannot be made to conform to the surface without wrinkling, the surface is of double curvature.
REPAIRS TO SINGLE CURVATURE PLYWOOD SKIN. Repairs to single curvature plywood skin may usually be formed from flat plywood, either by bending it dry or after soaking it in hot water. The degree of curvature to which a piece of plywood can be bent will depend upon the direction of the grain and the thickness. Table 1-2 is a guide
Par 1-49 Page 1-85
1. AFTER INSERTED WEB HAS BEEN BONDED IN PLACE, BOND COVER STRIPS OVER ENTIRE
LENGTH OF WEB SPLICE JOINTS.
2. SECTIONAL SHAPE OF FILLER BLOCKS MUST CONFORM EXACTLY TO TAPER OF SPAR. THEY MUST
NOT BE TOO TIGHTLY FITTED, FOR WEDGING ACTION WILL LOOSEN EXISTING BONDS OF WEBS TO FLANGES. IF TOO LOOSELY FITTED, CRUSHING OF WEB WILL OCCUR WHEN CLAMPING.
3. DIRECTION OF FACE GRAIN OF INSERTED WEB SECTION AND COVER STRIPS TO BE SAME AS ORIGINAL WEB.
FIGURE 1-9. Method of splicing box spar webs.
Par 1-49 Page 1-86
FIGURE 1-10. Method of reinforcing a longitudinal crack and/or local damage in a solid spar.
for determining which process of bending should be used for the curvature being considered.
Plywood, after softening, may be bent on a cold ventilated form, or it may be bent over the leading edge near the area being patched if space permits. In either method the repair part should be allowed to dry completely on the form. When bending plywood over a leading edge, drying may be hastened by laying a piece of coarse burlap over the leading edge before using it as a bending form. To speed drying, a fan may be used to circulate air around the repair part.
In bending pieces of small radii or to speed up the bending of a large number of parts of the same curvature, it may be necessary to use a heated bending form. The surface temperature of this form may be as high as 149 °C (300 ºF), if necessary, without danger of damage to the plywood. The plywood should be left on the heated form only long enough to dry to room conditions.
REPAIRS TO DOUBLE CURVATURE PLYWOOD SKIN. The molded plywood necessary for a repair to a damaged plywood skin of double curvature cannot be made from flat plywood unless the area to be repaired is very small or is of exceedingly slight double curvature; therefore, molded plywood of the proper curvature must be onhand before the repair can be made. If molded plywood of the proper curvature is available, the repair may be made using the same procedure as on single curvature skins.
12F RECOMMENDED 10F MINIMUM
DAMAGED AREA
ORIGINAL GUSSET
PLYWOOD-
SPRUCE OR
BASSWOOD AT A SPAR * 4A → ЗА
- 5A - →C→ • 5A ~ AT TRAILING EDGE 10A A,B,C,D,E,F,G = ORIGINAL DIMENSIONS.
REINFORCEMENT PLATES
SHALL BE PLYWOOD AT A JOINT TO TRUSS MEMBERS THE DIRECTION OF THE GLUED AND NAILED.
FACE GRAIN MUST BE
THE SAME AS ORIGINAL GUSSET.
— ЗА • 10A - ЗА - з‡
BETWEEN JOINTS FIGURE 1-11. Repair of wood ribs.
Par 1-50 Page 1-87
SEE FIGURE 1-11 FOR - REPAIR REPAIR OF CAP STRIPS. DAMAGE
SEE (D) (А) ЗА - ЗА SEE FIGURE 1-11 FOR DAMAGE REPAIR OF CAP STRIPS. REPAIR (B) SEE FIGURE 1-11 FOR
REPAIR OF CAP STRIPS REPAIR DAMAGE - (C)
•12A, BA COINIMENDED 6A 6 A (D)
A-A B-B
PLAND PACE GRAIN DERECTTON AS THIGINESS FIGURE 1-12. Typical wing compression rib repairs.
Par 1-50 Page 1-88
Par 1-50 Page 1-89 TABLE 1-2. Minimum recommended bend radii for aircraft plywood.
10 PERCENT MOISTURE
CONTENT, BENT ON COLD
MANDRELS
THOROUGHLY SOAKED IN HOT
WATER AND BENT ON COLD
MANDRELS
PLYWOOD
CHARACTERISTICS AT 90 º TO A T 0 º OR 45º
FACE GRAIN
T O F A C E
GRAIN AT 90 º TO A T 0º0R 45°
FACE GRAIN
TO FACE
GRAIN
THICKNESS (INCHES) NUMBER
OF PLIES MINIMUM BEND RADIUS (INCHES) .035 3 2.0 1.1 0.5 0.1 .070 3 5.2 3.2 1.5 0.4 .100 3 8.6 5.2 2.6 0.8 .125 3 12 7.1 3.8 1.2 .155 3 16 10 5.3 1.8 .185 3 20 13 7.1 2.6 .160 5 17 11 6 2 .190 5 21 14 7 3 .225 5 27 17 10 4 .250 5 31 20 12 5 .315 5 43 28 16 7 .375 5 54 36 21 10
TYPES OF PATCHES. There are four types of patches: splayed patch, surface (or overlay) patch, scarf patch, and plug patch. They are all acceptable for repairing plywood skins.
Splayed Patch. Small holes with their largest dimensions not over 15 times the skin thickness, in skins not more than 1/10 inch in thickness, may be repaired by using a circular splayed patch as illustrated in figure 1-13. The term “splayed” is used to denote that the edges of the patch are tapered, but the slope is steeper than is allowed in scarfing operations.
Lay out the patch according to figure 1-13. Tack a small piece of plywood over the hole for a center point and draw two circles with a divider, the inner circle to be the size of the hole and the outer circle marking the limits of the taper. The difference between the radii is 5T (5 times the thickness of the skin). If one leg of the dividers has been sharpened to a chisel edge, the dividers may be used to cut the inner circle.
Taper the hole evenly to the outer mark with a chisel, knife, or rasp.
Prepare a circular tapered patch to fit the prepared hole, and bond the patch into place with face-grain direction matching that of the original surface.
Use waxed paper or plastic wrap, (cut larger than the size of the patch) between the patch and the plywood pressure plate. This prevents excess adhesive from bonding the pressure plate to the skin. Center the pressure plate carefully over the patch.
AC 43.13-1B
Par 1-36 Page 1-90 As there is no reinforcement behind this patch, care must be used so that pressure is not great enough to crack the skin. On horizontal surfaces, weights or sandbags will be sufficient. On patches too far from any edge for the use of standard hand clamps, jaws of greater length may be improvised.
Table 1-2, columns (1) and (3), may also be used for determining the maximum thickness of single laminations for curved members.
Fill, sand, and refinish the patch.
Surface Patch. Plywood skins that are damaged between or along framing members may be repaired by surface or overlay patches as shown in figure 1-14.
Surface patches located entir ely aft of the 10 percent chord line, or which wrap around the leading edge and terminate aft of the 10 percent chord line, are permissible. Surface patches may have as much as a 50 inch perimeter and may cover as much as 1 frame (or rib) space. Trim the damage d skin to a rectangular or triangular shape and round the corners. The radius of rounded corners must be at least 5 times the skin thickness. Bevel the forward edges of patches located entirely aft of the 10 percent chord line to 4 times the skin thickness. The face-gr ain direction must be the same as the original skin . Cover completed surface patches with fabric to match surrounding area. The fabric must overlap the original fabric at least 2 inches.
Scarf Patch. A properly prepared and inserted scarf patch is the best repair for damaged plywood skins and is preferred for most skin repairs. Figure 1-15 shows the details and dimensions to be used when installing typical scarf skin patches, wh en the back of the skin is accessible. Follow figure 1- 16 when the back of the skin is not accessible. The scarf slope of 1 in 12, shown in both figures, is the steepest slope permitted for all kinds of plywood. If the radius of curvature of the skin at all points on the trimmed opening is greater than 100 times the skin thickness, a scarf patch may be installed.
Scarf cuts in plywood may be made by hand plane, spoke shave, scraper, or accurate sandpaper block.
Rasped surfaces, except at the corners of scarf patches and sawn surfaces, are not recommended as they are likely to be rough or inaccurate.
Nail strip or small screw clamping is often the only method available for bonding scarf joints in plywood skin repairs. It is essential that all scarf joints in plywood be backed with plywood or solid wood to provide adequate nail holding capacity.
The face-grain direction of the plywood patch must be the same as that of the original skin.
If the back of a damaged plywood skin is accessible (such as a fuselage skin), it should be repaired with a scarf patch, following the details shown in figure 1-15. Whenever possible, the edges of the patch should be supported as shown in section C-C of figure 1-15. When the damage follows or extends to a framing member, the scarf may be supported as shown in section B-B of figure 1-15. Damages that do not exceed 25 times the skin thickness in diameter after being trimmed to a circular shape and are not less than 15 times the skin thickness to a framing member, may be repaired as shown in figure 1-15, section D-D.
The backing block is carefully shaped from solid wood and fitted to the inside surface of the skin, and is temporarily held in place with nails.
Use waxed paper or plastic wrap to prevent bonding of the backing block to the skin.
Par 1-51 Page 1-27
FIGURE 1-13. Splayed patch.
A hole, the exact size of the inside circle of the scarf patch, is made in the block, and is centered over the trimmed area of damage.
The block is removed, after the adhesive on the patch has set, leaving a flush surface to the repaired skin.
Steps in making a scarf patch when the back of the skin is not accessible are as follows:
After removing damaged sections, install backing strips, as shown in figure 1-16, along all edges that are not fully backed by a rib or a spar. To prevent warping of the skin, backing strips should be made of a soft-textured plywood, such as yellow poplar or spruce rather than solid wood. All junctions between backing strips and ribs or spars should have the end of the backing strip supported by a saddle gusset of plywood.
If needed, nail and bond the new gusset plate to rib. It may be necessary to remove and replace the old gusset plate with a new saddle gusset, or it may be necessary to nail a saddle gusset over the original gusset.
Attach nailing strips to hold backing strips in place while the adhesive sets. Use a bucking bar, where necessary, to provide support for nailing. After the backing strips are fully bonded, install the patch.
Plug Patch. Either oval or round plug patches may be used on plywood skins provided the damage can be covered by thepatches whose dimensions are given in figure 1-17 and figure 1-18. The plug patch is strictly a skin repair, and should be used only for damage that does not involve the supporting structure under the skin.
The face-grain direction of the finished patch must match the surrounding skin.
Steps in making an oval plug patch are as follows:
Explore the area about the hole to be sure it lies at least the width of the oval