Boeing MD-11F
Service difficulty reports · 31,322
Newest first. General aviation reporting is voluntary.
Query with SQL
duckdb -csv -c "SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = 'MD11F' ORDER BY difficulty_date DESC"
Prints the whole list as CSV. It reads the release’s Parquet files over HTTPS, so there’s nothing to download first. Install DuckDB to run it.
SELECT sdr_id, difficulty_date, n_number, aircraft_make, aircraft_model, part_name, part_condition, jasc_code, discrepancy FROM 'https://openairdocs.org/data/latest/faa_service_difficulty_report.parquet' WHERE aircraft_model_key = 'MD11F' ORDER BY difficulty_date DESC
Run it at the DuckDB prompt, or in any tool that reads Parquet over HTTPS. More ways to query the release are on Use the data.
SDR 08FDEA01320Fitting · crackedMAIN DECK CARGO DOOR LOWER JAMB SPOOL FITTING NR 6 FOUND THIRD LAYER CRACK INDICATION AFTER BORE TO MAXIMUM 0.519". REMOVED AND REPLACED PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01319Fitting · crackedMAIN DECK CARGO DOOR LOWER JAMB SPOOL FITTING NR 4 FOUND THIRD LAYER CRACK INDICATION AFTER BORE TO MAXIMUM 0.519". REMOVED AND REPLACED PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01318Fitting · crackedMAIN DECK CARGO DOOR LOWER JAMB SPOOL FITTING NR 3 FOUND THIRD LAYER CRACK INDICATION AFTER BORE TO MAXIMUM 0.519". REMOVED AND REPLACED PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01317Fitting · crackedMAIN DECK CARGO DOOR LOWER JAMB SPOOL FITTING NR 2 FOUND THIRD LAYER CRACK INDICATION AFTER BORE TO MAXIMUM 0.519". REMOVED AND REPLACED PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01316Fitting · crackedMAIN DECK CARGO DOOR LOWER DOOR JAMB SPOOL FITTING NR 1 FOUND THIRD LAYER CRACK INDICATION AFTER BORE TO MAXIMUM 0.519". REMOVED AND REPLACED PER SRM 51-31-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR UPS08M51975Wire · brokenEMERGENCY LIGHTS INOP. BROKEN WIRE AT BATTERY CONNECTOR. REPAIRED WIRING IAW SWPM 20-41. OPS CHECKED NORMAL.SDR 08FDEA01314Skin · corrodedL3 DOOR CUT-OUT LOWER AFT CORNER FOUND CORRODED. COMPLIED WITH EA 1-5310-112608. CLASSIFIED AS MAJOR REPAIR AS PER FEDEX GMM 6-2-100.SDR UPS08M52546Stringer · crackedINSPECTION TYPE:C RT WING FUEL TANK UPPER NR 13 STRINGER END SUSPECT CRACK. HFEC INSP C/O AND FOUND CRACK APPROX 8 INCH. NR 13 STR END SPLICE REMOVED. STR CRACKED AREA CUT-OFF AND REMOVED. HFEC C/O ON TRIMMED EDGE AND FOUND NO CRACK EVIDENT. REPAIR STR, SSDR UPS08M53543Spar · corrodedINSPECTION TYPE:N/A VERTICAL STABILIZER FRONT SPAR RT CUTOUT AT STA ZFS 516-443 APPROX FOUND MINOR CORROSION AS MARKED. VERTICAL STABILIZER FRONT SPAR RT CUTOUT STA ZFS 516.443 APPROX MINOR CORROSION REMOVED AND REPROTECTED AS PER SRM 51-21-01 VOL II REV 35, SDR 08FDEA01278Skin · cracked08 EACH FASTENER HOLES FOUND WITH CRACK INDICATION DURING HFEC OPEN HOLE INSPECTION AT RIGHT WING LOWER SKIN ACCESS DOOR CUTOUT BETWEEN STA XORS = 690 AND STA XORS = 700. REPAIR CARRIED OUT AS PER EA 1-5710-120551, REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-10SDR 08FDEA01277Access Panel · corroded06 EACH FASTENER HOLES FOUND WITH CRACK INDICATION DURING HFEC OPEN HOLE INSPECTION AT LEFT WING LOWER SKIN ACCESS DOOR CUTOUT BETWEEN STA XORS = 690 AND STA XORS = 700. REPAIR CARRIED OUT AS PER EA 1-5710-120550, REPAIR CLASSIFIED AS MINOR PER GMM 6-2-100SDR 08FDEA01276Seat Track · corrodedMAIN DECK SEAT TRACK INBOARD FLANGE AT STA 1481 TO STA 1515, X = -75 FOUND CORROSION. REPAIRED BY SECTIONAL REPLACEMENT PER SRM 53-70-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01275Seat Track · corrodedMAIN DECK SEAT TRACK FLANGE AT STA 1395, X = -75 FOUND EXFOLIATION CORROSION. REPAIRED BY SECTIONAL REPLACEMENT PER SRM 53-70-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01274Seat Track · corrodedMAIN DECK SEAT TRACK FLANGE AT STA 1470, X = -75 FOUND EXFOLIATION CORROSION. REPAIRED BY SECTIONAL REPLACEMENT PER SRM 53-70-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR 08FDEA01273Seat Track · corrodedMAIN DECK SEAT TRACK FLANGE BELOW FLOOR PANEL NR 272HF AT STA 5-73, X = -8 HAS EXFOLIATION CORROSION. REPAIRED BY SECTIONAL REPLACEMENT PER SRM 53-70-00 FIGURE 1 VOLUME I. REPAIR CLASSIFIED AS MAJOR PER GMM 6-2-100.SDR WRLA2008040Hinge Fitting · crackedDURING C-CHECK INSPECTION FOUND LEFT OUTBOARD FLAP CENTER BOX INBOARD AFT HINGE SUPPORT FITTING CRACKED. REMOVED AND REPLACED HINGE WITH NEW PARTS IAW MD11 SRM VOL.II 51-33-01 REV.40SDR 08FDEA01256Stringer · crackedRIGHT WING, AFTER PANEL REMOVAL FOUND LEADING EDGE STRINGER CRACK AT XOS 667. REPAIR CARRIED OUT PER EA 1-5710-120544, REPAIR CLASSIFIED AS MINOR PER GMM 6-2-100.SDR 08FDEA01255Skin · dentedLEFT WING, INBOARD FLAP LOWER SKIN FOUND WITH DENT AT STA XIFH 299. DENT AREA MEASURED AND FOUND OUT OF LIMIT PER SRM 57-10-00 FIGURE 17 VOLUME I. REPAIR CARRIED OUT PER SRM 57-10-00 FIGURE 3 VOLUME I. REPAIR CLASSIFIED AS MINOR PER GMM 6-2-100.SDR 08FDEA01253Skin · dentedRIGHT WING, INBOARD FLAP LOWER SURFACE FOUND DENTS AT XIFH 150. DENTED AREA MEASURED FOUND OUT OF LIMIT PER SRM 57-10-00 FIGURE 17 VOLUME I. DEPTH = 0.048" AND DIAMETER = 0.5". REPAIR CARRIED OUT PER SRM 57-10-00 FIGURE 3 VOLUME I. REPAIR CLASSIFIED AS MINOSDR 08FDEA01250Access Panel · crackedRIGHT WING, LEADING EDGE LOWER SURFACE ACCESS PANEL 619CB INBOARD CORNER CUTOUT AREA FOUND CRACK. REPAIR CARRIED OUT PER SRM 57-10-00 FIGURE 21 VOLUME I. FABRICATED FILLER AND DOUBLER INSTALLED AS PER SRM 51-33-01 VOLUME II. REPAIR CLASSIFIED AS MAJOR PER GMMSDR WRLA2008032Stiffener · crackedDURING C-CHECK INSPECTION FOUND FLOORBEAM SUPPORT 5 EA STIFFENERS CRACKED STA Y=1841 X=-9.5, X=26, X=30.5, X=38, X=-38. REPLACED STIFFENERS PER MD11 SRM 51-35-01 VOL II REV 40.SDR UPS08M52211Frame · crackedINSPECTION TYPE:4C CRACK AT FRAME TO FLOOR BRACKET AT FS 1258 RBL 106. REMOVED, FABRICATED, AND INSTALLED FRAME PER EO MD11-5310-29275-A DAC DWG AEA7605, MD-11 SRM 53-33-01, AND SAA EA 011-5310-01-A1340.SDR UPS08M52208Seat Track · corrodedINSPECTION TYPE:4C AT STA 475 FROM 0 BUTTLINE TO OUTBOARD AFT OF R1 DOOR AREA SEAT TRACK FOR RCB PANEL IS CRACKED (EXFOLIATED CORROSION). REMOVED, FABRICATED, AND REPLACED SEAT TRACK PER DWG WSP0826, SAA TRAVELER 79598420001, AND SRM 51-31-01.SDR UPS08M52207Seat Track · corrodedINSPECTION TYPE:2C RCB LEFT FLOOR PANEL SUPPORT AT STA 495 CRACKED AND BUCKLING ON INBOARD SUPPORT AS WELL (EXFOLIATED CORROSION). REMOVED, FABRICATED, AND REPLACED SEAT TRACK PER DWB WSP0826 SAA TRAVELER 79598410001, AND SRM 51-33-01, 51-21-00.SDR UPS08M52671Skin · corrodedINSPECTION TYPE-C, CORROSION AROUND FASTENER HEADS ON O/WING CTR FUEL TANK UPPER SURFACE AT STA 1229 X=-87 TO -107. LOCK FASTENER ON AFFECTED AREA REMVD FOR ACCESS. CORROSION REMOVED, MEASURED THK: 0.170", MAT'L REMOVED:0.067", MAT'L REMN:0.103". FOUND OUT SDR UPS08M52204Skin · damagedINSPECTION TYPE:C LIGHTNING STRIKE OUTER FUSE SKIN, FS 1119 STR 1. DISPLACED INSULATION FOR ACCESS IAW AMM 25-82-01-4 2. REMOVED DAMAGED FASTENERS IAW SRM 51-35-01, BURN AROUND COUNTER SINK & OUTER SKIN DIA OR LENGTH: .420" DEEP: .060"D, NORMAL DIA OF CSK ISSDR CO1Y200800002Structure · corrodedAT HORIZONTAL STABILIZER CTR SECTION, FOUND CORROSION INSIDE BARREL NUT HOLE NR 36 LT HORIZ STAB.SDR UPS08M52670Hinge · corrodedINSPECTION TYPE-C, RT WING OB FLAP IB HINGE (FLAP MOUNTED) UPPER MOUNTING POINT FWD OB NR 2 BORE HOLE FOUND CORRODED AS MARKED. CORRODED IN AFFECTED AREA REMOVED. ORG DIA 0.599", FINAL DIA 0.6725". FPI C/O ON REWORK AREA & FOUND NO CORROSION EVDNT. BORE FINASDR UPS08M52631Bushing · corrodedINSPECTION TYPE-C, LT WING IB FLAP OB HINGE PIVOT POINT IB LUG BUSHING FOUND CORRODED. CORROSION REMOVED EXCEED LIMIT CMM 57-52-03 PG 442-444 R60 ORIG DIA 1.188, FINAL 1.257 MAX ALLOWABLE 1.220. FPI C/O DACNDTSPMR13PT8 NO CORR EVIDENT. RW K AREA PORTECTED, PSDR UPS08M52630Bushing · corrodedINSPECTION TYPE-C, LT WING IB FLAP OB HINGE PIVOT POINT OB LUG BUSHING FOUND CORRODED. CORROSION REMOVED EXCEED LIMIT CMM 57-52-03PG442-444R60 ORIG DIA 1.187" FINAL 1.258" MAX ALLOWABLE 1.220". FPI C/O NDT SPM R13PT8 NO CORROSION EVIDENT. AREA PROTECTED & PASDR UPS08M52229Structure · crackedINSPECTION TYPE:4C LEFT WING LE ACCESS PANEL LANDING AT NR 9 SLAT TRACK CRACKED. FABRICATED AND INSTALLED REPAIR DOUBLER IAW MD-11 SRM 57-10-00 FIG.18.SDR UPS08M52192Seat Track · corrodedINSPECTION TYPE:C AFT CABIN - CORROSION IN SEAT TRACK CHANNEL AT STA 1841 X=107. CORROSION AT AFFECTED AREA REMOVED MATL THK:0.100" (CHANNEL) MATL REMOVED:0.05 0" (STA1841-1853), MATL REMN:0.050". FOUND OUT OF LIMIT. DISCREPANT SEA TRACK AT STA1831 X=107, TSDR UPS08M52041Skin · crackedINSPECTION TYPE:4C LEFT WING LE NR 14 SLAT TRACK CUT OUT CRACKED. CUT OUT DAMAGE, FABRICATED AND INSTALLED REPAIR FILLER AND DOUBLER IAW MD-11 SRM 57-10-00 FIG 21 AND 51-33-01.SDR UPS08M52040Skin · crackedINSPECTION TYPE:4C LEFT WING LE SKIN SPLICE STRAP XFS 669 CRACKED. REMOVED CRACKED SKIN SPLICE STRAP. FABRICATED AND INSTALLED REPLACEMENT SKIN SPLICE STRAP IAW DWG ARB3954 AND 51-33-01.SDR UPS08M52039Stringer · crackedINSPECTION TYPE:4C LEFT WING LE ACCESS PNL LANDING XOS 550 STRINGER CRACKED. FABRICATED AND INSTALLED REPAIR DOUBLER IAW MD-11 SRM 57-10-00 FIG 18 AND 51-33-01.SDR UPS08M52038Skin · crackedINSPECTION TYPE:4C RT WING LE ACCESS PNL LANDING AT SLAT TRACK FITTING 9 STRINGER CRACKED. REMOVED CRACKED STRINGER DOUBLER. FABRICATED AND INSTALLED REPLACEMENT STRINGER DOUBLER IAW DWG ARB1180 AND MD-11 SRM 51-33-01.SDR UPS08M52037Stringer · crackedINSPECTION TYPE:4C RT WING LE ACCESS PNL LANDING XOS 550 STRINGER DOUBLER CRACKED. FABRICATED AND INSTALLED REPAIR DOUBLER IAW MD-11 SRM 57-10-00 FIG 18 AND 51-33-01.SDR UPS08M52035Skin · crackedINSPECTION TYPE:4C RIGHT WING LE SKIN SPLICE STRAP XFS669 CRACKED. REMOVED CRACKED SPLICE STRAP, FABRICATED AND INSTALLED REPLACEMENT SPLICE STRAP IAW DWG ARB3954 AND MD-11 SRM 51-33-01.SDR UPS08M52034Skin · crackedINSPECTION TYPE:4C RIGHT WING LE SKIN SPLICE STRAP XFS791 CRACKED. REMOVED CRACKED SKIN SPLICE. FABRICATED AND INSTALLED REPLACEMENT SKIN SPLICE IAW DWG ARB3954 AND MD-11 SRM 51-33-01.SDR UPS08M52048Fitting · crackedINSPECTION TYPE:4C LEFT WING NR 16 SLAT TRACK IB FITTING CRACKED. REMOVED AND REPLACED NR 16 SLAT TRACK IB RIB FITTING IAW MD-11 SRM 51-31-01 AND 51-33-01.SDR UPS08M52047Fitting · crackedINSPECTION TYPE:4C RIGHT WING NR 16 SLAT TRACK FITTING IB CRACKED. REMOVED AND REPLACED NR 16 SLAT TRACK IB RIB FITTING IAW MD-11 SRM 51-31-01 AND 51-33-01.SDR 08FDEA01118Frame · dentedMAIN DECK LEFT FRAME AT BS 1721 S12L FOUND DENTED. REPAIRED AS PER SRM 53-30-00, FIG.1, VOL.1. INITIAL INSPECTION AT 14,500 CYCLES AND REPETITIVE INSPECTION AT 9,500 CYCLES TO BE CARRIED OUT AS PER SRM 53-30-00, FIG.1, VOL.1. REPAIR CLASSIFIED AS MAJOR ASDR 08FDEA01117Frame · chafedMAIN DECK LT FRAME AT STATION 535 , BETWEEN L23-24L, 1 CHAFED MARK FOUND. REPAIRED AS PER DRAWING SRZ-53-503. REPAIR CLASSIFIED AS MINOR AS PER GMM 6-2-100.SDR 08FDEA01116Frame · chafedMAIN DECK LEFT FRAME AT BS 535, BETWEEN L19-20L, 01 EACH CHAFED MARK FOUND NEAR 9G NET YOKE. REPAIRED AS PER DRAWING SRZ-53-503. REPAIR CLASSIFIED AS MINOR AS PER GMM 6-2-100.SDR 08FDEA01115Frame · dentedMAIN DECK LEFT FRAME AT STATION 1661, STRINGER 12 LEFT FOUND DENTED. REPAIRED AS PER SRM 53-30-00, FIG.1, VOL.1. INITIAL INSPECTION AT 14,500 CYCLES AND REPETITIVE INSPECTION AT 9,500 CYCLES TO BE CARRIED OUT AS PER SRM 53-30-00, FIG.1, VOL.1. REPAIR CLASSIFSDR 08FDEA01114Frame · dentedMAIN DECK RIGHT FRAME AT BS 1721 S12R FOUND DENTED. REPAIRED AS PER SRM 53-30-00, FIG.1, VOL.1. INITIAL INSPECTION AT 14,500 CYCLES AND REPETITIVE INSPECTION AT 9,500 CYCLES TO BE CARRIED OUT AS PER SRM 53-30-00, FIG.1, VOL.1. REPAIR CLASSIFIED AS MAJOR AS PSDR 08FDEA01113Frame · dentedMAIN DECK RIGHT FRAME AT STATION 1681, STRINGER 12 RIGHT FOUND DENTED. REPAIRED AS PER SRM 53-30-00, FIG.1, VOL.1. INITIAL INSPECTION AT 14,500 CYCLES AND REPETITIVE INSPECTION AT 9,500 CYCLES TO BE CARRIED OUT AS PER SRM 53-30-00, FIG.1, VOL.1. REPAIR CLASSSDR UPS08M52082Arm · damagedINSPECTION TYPE:2C 4 RUDDER PEDAL ARM ASSEMBLIES REQUIRE NDT FOR PREVIOUSLY DRILLED LOCK FASTENER HOLES. REMOVED LOCK FASTENER, PERFORMED FP INSPECTION, NO CRACKS NOTED, APPLIED ALODINE TO HOLES, INSTALLED HLT334-6-22 FASTENERS AND HL386-6 COLLARS AND MARKED SDR 08FDEA01087Skin · crackedLEFT WING LEADING EDGE ANTI-ICE TELESCOPIC DUCT DOOR CUT OUT CORNER SKIN CRACKED. REPAIRED AS PER SRM 57-10-00, FIGURE 43, VOLUME 1. THIS REPAIR CLASSIFIED AS MAJOR AS PER GMM 6-2-100.SDR 08FDEA01070Fitting · crackedMAIN DECK CARGO DOOR, LOWER JAMB FITTING FOUND NR 7 HOLE POSITION "C" "A", "B", ":D" CORRODED. COMPLIED WITH EA 1-5310-112602 PART 1. FITTING REMOVED AND REPLACED AS PER SRM 51-33-01 VOL.II. REPAIR CLASSIFIED AS MAJOR AS PER GMM 6-2-100.
Back to Boeing MD-11F