AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 119–130
Page 131Open in PDF

will impose so much stress on the surface of the plastic that tiny fissures or cracks, called crazing, will form.

3-21. HEATING. Before heating any trans­ parent plastic material, remove all of the masking paper and adhesive from the sheet. If the sheet is dusty or dirty, wash it with clean water and rinse it well. Dry the sheet thor­ oughly by blotting it with soft absorbent paper towels.

NOTE: Wear cotton gloves when handling the plastic to eliminate finger marks on the soft surface.

a. For the best results when hot-forming acrylics, use the temperatures recommended by the manufacturer. A forced-air oven should be used −one that is ca­ pable of operating over a temperature range of 120 to 374 °F (49 to 190 °C). If the part gets too hot during the forming process, bubbles may form on the surface and impair the optical qualities of the sheet.

b. For uniform heating, it is best to hang the sheets vertically by grasping them by their edges with spring clips and suspending the clips in a rack. (See figure 3-17.) If the piece is too small to hold with clips, or if there is not enough trim area, lay the sheets on shelves or racks covered with soft felt or flannel. Be sure there is enough open space to allow the air to circulate around the sheet and heat it evenly.

c. Small forming jobs, such as landing light covers, may be heated in a kitchen baking oven. Infrared heat lamps may be used if they are arranged on 7-or 8-inch centers and enough of them are used in a bank to heat the sheet evenly. Place the lamps about 18 inches from the material.

FIGURE 3-17. Hanging of acrylic sheets.

d. Never use hot water or steam directly on the plastic to heat it, because this will likely cause the acrylic to become milky or cloudy.

3-22. FORMS. Heated acrylic plastic will mold with almost no pressure, so the forms used can be of very simple construction.

Forms made of pressed wood, plywood, or plaster are adequate to form simple curves, but reinforced plastic or plaster may be needed to shape complex or compound curves.

a. Since hot plastic conforms to any waviness or unevenness, the form used must be completely smooth. To ensure this, sand the form and cover it with soft cloth such as outing flannel or billiard felt.

b. The mold should be large enough to extend beyond the trim line of the part, and provisions should be made for holding the hot plastic snug against the mold as it cools.

c. A mold can be made for a complex part by using the damaged part itself. If the part is broken, tape the pieces together, wax or grease the inside so the plaster will not stick to it, and support the entire part in sand. Fill the part with plaster and allow it to harden, and Page 3-16 Par 3-20

Page 132Open in PDF

then remove it from the mold. Smooth out any roughness and cover it with soft cloth. It is now ready to use to form the new part.

3-23. FORMING METHODS. (See ta­ ble 3-1.)

a. Simple Curve Forming. Heat the plastic material to the recommended tempera­ ture, remove it from the heat source, and care­ fully drape it over the prepared form. Care­ fully press the hot plastic to the form and ei­ ther hold or clamp the sheet in place until it cools. This process may take from ten minutes to one-half hour. Do not force-cool it.

b. Compound-Curve Forming. This type of forming is normally used for such parts as canopies or complex wingtip light covers, and it requires a great deal of specialized equipment. There are four commonly used methods, each having its advantages and dis­ advantages.

c. Stretch Forming. Preheated acrylic sheets are stretched mechanically over the form in much the same way as is done with the simple curved piece. Special care must be taken to preserve uniform thickness of the material, since some parts will have to stretch more than others.

d. Male And Female Die Forming. This requires expensive matching male and female dies. The heated plastic sheet is placed be­ tween the dies which are then mated. When the plastic cools, the dies are opened.

e. Vacuum-Forming Without Forms.

Many aircraft canopies are formed by this method. In this process a clamp with an opening of the desired shape is placed over a vacuum box and the heated sheet of plastic is clamped in place. When the air in the box is evacuated, the outside air pressure will force the hot plastic through the opening and form the concave canopy. It is the surface tension of the plastic that shapes the canopy.

f. Vacuum-Forming With A Female Form. If the shape needed is other than that which would be formed by surface tension, a female mold, or form must be used. It is placed below the plastic sheet and the vacuum pump is connected. When air from the form is evacuated, the outside air pressure will force the hot plastic sheet into the mold and fill it.

g. Sawing And Drilling.

(1) Several types of saws can be used with transparent plastics, however circular saws are the best for straight cuts. The blades TABLE 3-1. Typical temperatures for forming acrylic sheets.

Thickness of sheet (in.) 0.125 0.250 0.125 0.250 Type of forming Regular acrylic plastic.

MIL-P-6886 Heat-resistant acrylic plastic, MIL-P-5425, and craze-resistant acrylic plastic, MIL-P-8184 °C °F °C °F °C °F °C °F Simple curve 113 235 110 230 135 275 135 275 Stretch forming (dry mold cover) 140 284 135 275 160 320 150 302 Male and female forming 140 284 135 275 180 356 170 338 Vacuum forming without form 140 284 135 275 150 302 145 293 Vacuum forming with female form 145 293 140 284 180 356 170 338 Par 3-22 Page 3-17

Page 133Open in PDF

should be hollow -ground or have some set to prevent binding. After the teeth are set, they should be side -dressed to produce a smooth edge on the cut. Band saws are recommended for cutting flat acrylic sheets when the cuts must be curved or where the sheet is cut to a rough dimension to be trimmed later. Close control of size and shape may be obtained by band sawing a piece to within 1/16 inch of the desired size, as marked by a scribed line on the plastic, and then sanding it to the correct size with a drum or belt sander.

(2) Unlike soft metal, acrylic plastic is a very poor conductor of heat. Make provisions for removing the heat when drilling. Deep holes need cooling, and a water-soluble cutting oil is a satisfactory coolant since it has no ten­ dency to attack the plastic.

(a) The drill used on acrylics must be carefully ground and free from nicks and burrs that would affect the surface finish. Grind the drill with a greater included angle than would be used for soft metal. The rake angle should be zero in order to scrape, not cut. (See fig­ ure 3-18.)

FIGURE 3-18. Drill having an included angle of approximately 150°, used to drill acrylic plastics.

(b) The patented Unibit (see fig­ ure 3-19) is good for drilling small holes in aircraft windshields and windows. It can cut holes from 1/8-to 1/2 −inch in 1/32 −inch in­ crements and produces good smooth holes with no stress cracks around their edges.

FIGURE 3-19. Unibit drill for drilling acrylic plastics.

h. Polymerizable Cements. Polymeri­ zable cements are those in which a catalyst is added to an already thick monomerpolymer syrup to promote rapid hardening. Ce­ ment PS-30 and Weld -On 40 are polymeri­ zable cements of this type. They are suitable for cementing all types of PLEXIGLAS acrylic cast sheet and parts molded from PLEXIGLAS molding pellets. At room temperature, the cements harden (polymerize) in the container in about 45 minutes after mixing the compo­ nents. They will harden more rapidly at higher temperatures. The cement joints are usually hard enough for handling within 4 hours after assembly. The joints may be machined within 4 hours after assembly, but it is better to wait 24 hours.

(1) PS-30 and Weld -On 40 joints retain excellent appearance and color stability after outdoor exposure. These cements produce clear, transparent joints and should be used when the color and appearance of the joints are important.

(2) PS-30 and Weld -On 40 should be used at temperatures no lower than 65 °F. If cementing is done in a room cooler than 65 °F, it will require a longer time to harden and the joint strength will be reduced.

(a) The cement should be prepared with the correct proportions of components as given in the manufacturer’s instructions and thoroughly mixed, making sure neither the mixing container nor mixing paddle adds color or affects the hardening of the cement.

Page 3-18 Par 3-23

Page 134Open in PDF

Clean glass or polyethylene mixing containers are preferred.

(b) Because of their short pot life (approximately 45 minutes) Cement PS-30 and Weld-On 40 must be used quickly once the components are mixed. Time consumed in preparation shortens the effective working time, making it necessary to have everything ready to be cemented before the cements are mixed. For better handling pour cement within 20 minutes of mixing.

(c) For maximum joint strength, the final cement joint should be free of bubbles. It will usually be sufficient to allow the mixed cement to stand for 10 minutes before ce­ menting to allow bubbles to rise to the surface.

(See figure 3-20.)

FIGURE 3-20. Applying pressure to acrylic plastics.

(d) The gap joint technique can only be used with colorless PLEXIGLAS acrylic or in cases in which joints will be hidden. If in­ conspicuous joints in colored PLEXIGLAS acrylic are needed, the parts must be fitted closely, using closed V groove, butt, or arc joints.

(3) Cement forms or dams may be made with masking tape as long as the adhesive sur­ face does not contact the cement. This is easily done with a strip of cellophane tape placed over the masking tape adhesive. The tape must be chosen carefully. The adhesive on ordinary cellophane tape prevents the cure of PS-30 and Weld-On 40. Before actual fab­ rication of parts, sample joints should be tried to ensure that the tape system used will not harm the cement. Since it is important for all of the cement to remain in the gap, only con­ tact pressure should be used.

(4) Bubbles will tend to float to the top of the cement bead in a gap joint after the ce­ ment is poured. These cause no problem if the bead is machined off. A small wire (not cop­ per), or similar objects may be used to lift some bubbles out of the joint; however, the cement joint should be disturbed as little as possible.

(5) Polymerizable cements shrink as the cement hardens. Therefore, the freshly poured cement bead should be left above the surfaces being cemented to compensate for the shrink­ age. If it is necessary for appearances, the bead may be machined off after the cement has set.

3-24. REPAIR OF PLASTICS. Replace, rather than repair extensively damaged trans­ parent plastic, whenever possible, since even a carefully patched part is not the equal of a new section, either optically or structurally. At the first sign of crack development, drill a small hole with a # 30 or a 1/8-inch drill at the ex­ treme ends of the cracks as shown in fig­ ure 3-21. This serves to localize the cracks and to prevent further splitting by distributing the strain over a large area. If the cracks are small, stopping them with drilled holes will usually suffice until replacement or more per­ manent repairs can be made. The following repairs are permissible; however, they are not to be located in the pilot’s line of vision during landing or normal flight.

Par 3-23 Page 3-19

Page 135OCROpen in PDF

ALL THE STRAINS WHICH ORIGINALLY CAUSED

THE CRACK ARE CONCENTRATED AT POINT A - TENDING TO EXTEND THE CRACK. THEREFORE DRILL, WITH A #30 OR 1/8" DRILL BIT, A SMALL HOLE AT END OF THE CRACK POINT A1) TO DISTRIBUTE THE STRAIN OVER A WIDER AREA.

EACH CRACK OCCURRING AT ANY HOLE OR TEAR IS DRILLED IN SAME MANNER.

FIGURE 3-21. Stop-drilling cracks.

a. Surface Patch. If a surface patch is to be installed, trim away the damaged area and RFACE PATCI round all corners. Cut a piece of plastic of sufficient size to cover the damaged area and ex- STOP CRÁCK DRILLED tend at least 3/4 inch on each side of the crack or hole. Bevel the edges as shown in figure 3-22. If the section to be repaired is SURFACE PATCH FOR CRACKS BEVELED EDGE curved, shape the patch to the same contour by heating it in an oil bath at a temperature of IRFACE PATCH 248 to 302 °F, or it may be heated on a TRIM DAMAGED AREA AND ROUND ALL CORNERS hot-plate until soft. Boiling water should not CORNER HARP be used for heating. Coat the patch evenly with plastic solvent adhesive and immediately place it over the hole. Maintain a uniform SURFACE PATCH FOR IRREGULAR SHAPED DAMAGE / 'EDGE BEVELED pressure of 5 to 10 psi on the patch for a minimum of 3 hours. Allow the patch to dry 24 to 36 hours before sanding or polishing.

ROUI

b. Plug Patch. When using inserted patches to repair holes in plastic structures, BEVELED EDGE trim the holes to a perfect circle or oval and SURFACE PATCH FOR ROUND HOLES ' bevel the edges slightly. Make the patch slightly thicker than the material being FIGURE 3-22. Surface patches.

Page 3-20 Par 3-24

Page 136Open in PDF

repaired and similarly bevel its edges. Install patches in accordance with figure 3-23. Heat the plug until soft and press it into the hole without cement and allow to cool to make a perfect fit. Remove the plug, coat the edges with adhesive, and then reinsert in the hole.

Maintain a firm light pressure until the cement has set. Sand or file the edges level with the surface, then buff and polish.

FIGURE 3-23. Plug patch repair.

3-25. CLEANING AND POLISHING TRANSPARENT PLASTIC. Plastics have many advantages over glass for aircraft use, but they lack the surface hardness of glass and care must be exercised while servicing the air­ craft to avoid scratching or otherwise damag­ ing the surface.

a. Clean the plastic by washing it with plenty of water and mild soap, using a clean, soft, grit-free cloth, sponge, or bare hands. Do not use gasoline, alcohol, benzene, acetone, carbon tetrachloride, fire extinguisher or deic­ ing fluids, lacquer thinners, or window clean­ ing sprays. These will soften the plastic and cause crazing.

b. Plastics should not be rubbed with a dry cloth since this is likely to cause scratches, and also to build up an electrostatic charge that attracts dust particles to the surface. If after removing dirt and grease, no great amount of scratching is visible, finish the plastic with a good grade of commercial wax. Apply the wax in a thin even coat and bring to a high polish by rubbing lightly with a soft cloth.

c. Do not attempt hand polishing or buffing until the surface is clean. A soft, open-type cotton or flannel buffing wheel is suggested. Minor scratches may be removed by vigorously rubbing the affected area by hand, using a soft clean cloth dampened with a mixture of turpentine and chalk, or by applying automobile cleanser with a damp cloth. Re­ move the cleaner and polish with a soft, dry cloth. Acrylic and cellulose acetate plastics are thermoplastic. Friction created by buffing or polishing too long in one spot can generate sufficient heat to soften the surface. This con­ dition will produce visual distortion and should be avoided.

3-26. REPLACEMENT PANELS. Use material equivalent to that originally used by the manufacturer of the aircraft for replace­ ment panels. There are many types of trans­ parent plastics on the market. Their properties vary greatly, particularly in regard to expan­ sion characteristics, brittleness under low Par 3-24 Page 3-21

Page 137Open in PDF

temperatures, resistance to discoloration when exposed to sunlight, surface checking, etc. In­ formation on these properties is in MIL-HDBK-17A, Plastics for Flight Vehicles, Part IITransparent Glazing Materials, avail­ able from the Government Printing Office (GPO). These properties are considered by aircraft manufacturers in selecting materials to be used in their designs and the use of substi­ tutes having different characteristics may result in subsequent difficulties.

3-27. INSTALLATION PROCEDURES.

When installing a replacement panel, use the same mounting method employed by the manufacturer of the aircraft. While the actual installation will vary from one type of aircraft to another, consider the following major prin­ ciples when installing any replacement panel.

a. Never force a plastic panel out of shape to make it fit a frame. If a replacement panel does not fit easily into the mounting, obtain a new replacement or heat the whole panel and reform. When possible, cut and fit a new panel at ordinary room temperature.

b. In clamping or bolting plastic panels into their mountings, do not place the plastic under excessive compressive stress. It is easy to develop more than 1,000 psi on the plastic by over-torquing a nut and bolt. Tighten each nut to a firm fit, then back the nut off one full turn (until they are snug and can still be rotated with the fingers).

c. In bolted installations, use spacers, collars, shoulders, or stop-nuts to prevent tightening the bolt excessively. Whenever such devices are used by the aircraft manufac­ turer, retain them in the replacement installa­ tion. It is important that the original number of bolts, complete with washers, spacers, etc., be used. When rivets are used, provide ade­ quate spacers or other satisfactory means to prevent excessive tightening of the frame to the plastic.

d. Mount plastic panels between rubber, cork, or other gasket material to make the in­ stallation waterproof, to reduce vibration, and to help to distribute compressive stresses on the plastic.

e. Plastics expand and contract consid­ erably more than the metal channels in which they are mounted. Mount windshield panels to a sufficient depth in the channel to prevent it from falling out when the panel contracts at low temperatures or deforms under load.

When the manufacturer’s original design per­ mits, mount panels to a minimum depth of 1-1/8 inch, and with a clearance of 1/8 inch between the plastic and bottom of the channel.

f. In installations involving bolts or rivets, make the holes through the plastic over­ size by 1/8-inch diameter and center so that the plastic will not bind or crack at the edge of the holes. The use of slotted holes is also recom­ mended.

3-28.  3-39. [RESERVED.] Page 3-22 Par 3-26

Page 138Open in PDF

SECTION 4. WINDSHIELDS, ENCLOSURES, AND WINDOWS

3-40. GENERAL. These repairs are appli­ cable to plastic windshields, enclosures, and windows in nonpressurized airplanes . For pressurized airplanes, replace or repair plastic elements in accordance with the manufac­ turer’s recommendation. When windshields and side windows made of acrylic plastics are damaged, they are usually replaced unless the damage is minor and a repair would not be in the line of vision. Repairs usually require a great deal of labor. Replacement parts are readily available, so replacement is normally more economical than repair.

a. Minor Repairs. There are times, how­ ever, when a windshield may be cracked and safety is not impaired. In that case, repairs can be made by stop-drilling the ends of the crack with a # 30 drill (1/8 inch) to prevent the con­ centration of stresses causing the crack to con­ tinue. Drill a series of number 40 holes a half-inch from the edge of the crack about a half-inch apart, and lace through these holes with brass safety wire (see figure 3-24) and seal with clear silicone to waterproof.

b. Temporary Repairs. One way to make a temporary repair is to stop-drill the ends of the crack, and then drill number 27 holes every inch or so in the crack. Use AN515-6 screws and AN365-632 nuts with AN960-6 washers on both sides of the plastic.

This will hold the crack together and prevent further breakage until the windshield can be properly repaired or replaced. (See fig­ ure 3-24.)

c. Permanent Repairs. Windshields or side windows with small cracks that affect only the appearance rather than the airworthi­ ness of a sheet, may be repaired by first stop-drilling the ends of the crack with a # 30 or a 1/8-inch drill. Then use a hypoder­ mic syringe and needle to fill the crack with polymerizable cement such as PS-30 or Weld-On 40, and allow capillary action to fill the crack completely. Soak the end of a 1/8-inch acrylic rod in cement to form a cush­ ion and insert it in the stop-drilled hole. Allow the repair to dry for about 30 minutes, and then trim the rod off flush with the sheet.

d. Polishing and Finishing. Scratches and repair marks, within certain limitations, can be removed from acrylic plastic. No sanding that could adversely affect the plas­ tic’s optical properties and distort the pilot’s vision should be done on any portion of a windshield.

(1) If there are scratches or repair marks in an area that can be sanded, they may be re­ moved by first sanding the area. Use 320- or 400-grit abrasive paper that is wrapped around a felt or rubber pad.

(2) Use circular rubbing motions, light pressure, and a mild liquid soap solution as a lubricant. After the sanding is complete, rinse the surface thoroughly with running water.

Then, using a 500-grit paper, continue to sand lightly. Keep moving to higher grit paper and sand and rinse until all of the sanding or repair marks have been removed.

(3) After using the finest abrasive pa­ per, use rubbing compound and buff in a cir­ cular motion to remove all traces of the sand­ ing.

e. Cleaning. Acrylic windshields and windows may be cleaned by washing them with mild soap and running water. Rub the surface with your bare hands in a stream of water. Follow with the same procedure but with soap and water. After the soap and dirt have been flushed away, dry the surface with a soft, clean cloth or tissue and polish it with a Par 3-40 Page 3-23

Page 139Open in PDF

FIGURE 3-24. Temporary repairs to cracked windshields or windows.

windshield cleaner especially approved for use on aircraft transparent plastics. These cleaners may be purchased through aircraft supply houses.

f. Waxing. A thin coating of wax will fill any minute scratches that may be present and will cause rain to form droplets that are easily blown away by the wind.

3-41. PROTECTION. Acrylic windshields are often called “lifetime” windshields, to dis­ tinguish them from those made of the much shorter-lived acetate material. However, even acrylic must be protected from the ravages of the elements.

a. When an aircraft is parked in direct sunlight, the windshield will absorb heat and will actually become hotter than either the in­ side of the aircraft or the outside air. The sun will cause the inside of a closed aircraft to be­ come extremely hot, and this heat is also ab­ sorbed by the plastic windshield.

b. To protect against this damage, it is wise to keep the aircraft in a hangar. If this is not possible, some type of shade should be provided to keep the sun from coming in direct contact with the windshield. Some aircraft owners use a close-fitting, opaque, reflective cover over the windshield. In many cases, this has done more harm than good. This cover may absorb moisture from the air and give off harmful vapors, and if it touches the surface of the plastic it can cause crazing or minute cracks to form in the windshield. Another hazard in using such a cover is that sand can blow up under the cover and scratch the plas­ tic.

3-42. WINDSHIELD INSTALLATION.

Aircraft windshields may be purchased either from the original aircraft manufacturer or from any of several FAA-PMA sources. These windshields are formed to the exact shape re­ quired, but are slightly larger than necessary so they may be trimmed to the exact size.

a. After removing the damaged windshield, clean all of the sealer from the grooves and cut the new windshield to fit. New wind­ shields are covered with either protective paper or film to prevent damage during handling or installation. Carefully peel back just enough of this covering to make the installation. The windshield must fit in its channels with about 1/8- to 1/4-inch clearance to allow for expan­ sion and contraction. If any holes are drilled in the plastic for screws, they should be about 1/8 inch oversize.

Page 3-24 Par 3-40

Page 140Open in PDF

b. Place the sealing tape around the edges of the windshield and install the wind­ shield in its frame. Screws that go through the windshield should be tightened down snug and then backed out a full turn, so the plastic can shift as it expands and contracts.

c. Do not remove the protective paper or film until the windshield is installed and all of the securing screws are in place.

3-43.  3-47. [RESERVED.] Par 3-42 Page 3-25 (and 3-26)

Page 141Open in PDF

CHAPTER 4. METAL STRUCTURE, WELDING, AND BRAZING

SECTION 1. IDENTIFICATION OF METALS

4-1. GENERAL. Proper identification of the aircraft structural material is the first step in ensuring that the continuing airworthiness of the aircraft will not be degraded by making an improper repair using the wrong materials.

a. Ferrous (iron) alloy materials are generally classified according to carbon con­ tent. (See table 4-1.)

TABLE 4-1. Ferrous (iron) alloy materials.

MATERIALS CARBON CONTENT Wrought iron Trace to 0.08% Low carbon steel 0.08% to 0.30% Medium carbon steel 0.30% to 0.60% High carbon steel 0.60% to 2.2% Cast iron 2.3% to 4.5%

b. The strength and ductility, or tough­ ness of steel, is controlled by the kind and quantity of alloys used and also by cold-working or heat-treating processes used in manufacturing. In general, any process that increases the strength of a material will also decrease its ductility.

c. Normalizing is heating steel to ap­ proximately 150 °F to 225 °F above the steel’s critical temperature range, followed by cooling to below that range in still air at ordinary tem­ perature. Normalizing may be classified as a form of annealing. This process also removes stresses due to machining, forging, bending, and welding. After the metal has been held at this temperature for a sufficient time to be heated uniformly throughout, remove the metal from the furnace and cool in still air. Avoid prolonging the soaking of the metal at high temperatures, as this practice will cause the grain structure to enlarge. The length of time required for the soaking temperature de­ pends on the mass of the metal being treated.

The soaking time is roughly ¼ hour per inch of the diameter of thickness (Ref: Military Tech Order (T.O.) 1-1A-9).

4-2. IDENTIFICATION OF STEEL STOCK. The Society of Automotive Engi­ neers (SAE) and the American Iron and Steel Institute (AISI) use a numerical index system to identify the composition of various steels.

The numbers assigned in the combined listing of standard steels issued by these groups repre­ sent the type of steel and make it possible to readily identify the principal elements in the material.

a. The basic numbers for the four digit series of the carbon and alloy steel may be found in table 4-2. The first digit of the four number designation indicates the type to which the steel belongs. Thus, “1” indicates a carbon steel, “2” a nickel steel, “3” a nickel chromium steel, etc. In the case of simple alloy steels, the second digit indicates the approximate per­ centage of the predominant alloying element.

The last two digits usually indicate the mean of the range of carbon content. Thus, the desig­ nation “1020” indicates a plain carbon steel lacking a principal alloying element and con­ taining an average of 0.20 percent

(0.18 to 0.23) carbon. The designation “2330” indicates a nickel steel of approximately 3 percent (3.25 to 3.75) nickel and an average of 0.30 percent, (0.28 to 0.33) carbon content.

The designation “4130” indicates a chromiummolybdenum steel of approximately 1 percent

(0.80 to 1.10) chromium, 0.20 percent

(0.15 to 0.25) molybdenum, and 0.30 percent

(0.28 to 0.33) carbon.

Par 4-5 Page 4-1

Page 142Open in PDF

b. There are numerous steels with higher percentages of alloying elements that do not fit into this numbering system. These include a large group of stainless and heat resisting al­ loys in which chromium is an essential alloy­ ing element. Some of these alloys are identi­ fied by three digit AISI numbers and many others by designations assigned by the steel company that produces them. The few exam­ ples in table 4-3 will serve to illustrate the kinds of designations used and the general al­ loy content of these steels.

c. “1025” welded tubing as per Specification MIL-T-5066 and “1025” seamless tubing con­ forming to Specification MIL-T-5066A are inter­ changeable.

4-3. INTERCHANGEABILITY OF STEEL TUBING .

a. “4130” welded tubing conforming to Specification MIL-T-6731, and “4130” seam-less tubing conforming to Specification MIL-T-6736 are interchangeable.

b. NE-8630 welded tubing conforming to Specification MIL -T-6734, and NE- 8630 seamless tubing conforming to Specification MIL-T-6732 are interchangeable.

4-4. IDENTIFICATION OF ALUMINUM .

To provide a visual means for identifying the various grades of aluminum and aluminum alloys, such metals are usually marked with symbols such as a Government Specification Number, the temper or condition furnished, or the commercial code marking. Plate and sheet are usually marked with specification numbers or code markings in rows approximately 5 inches apart. Tubes, bars, rods, and extruded shapes are marked with specification numbers or code markings at intervals of 3 to 5 feet along the length of each piece.

The commercial code marking consists of a number which identifies the particular compo­ sition of the alloy. In addition, letter suffixes (see table 4-4) designate the basic temper des­ ignations and subdivisions of aluminum alloys.

TABLE 4-2. Numerical system for steel identification.

TYPES OF STEELS NUMERALS

AND DIGITS Plain carbon steel 10XX Carbon steel with additional sulfur for easy machining.

11XX Carbon steel with about 1.75% manganese 13XX .25% molybdenum. 40XX 1% chromium, .25% molybdenum 41XX 2% nickel, 1% chromium, .25% molybdenum 43XX

1.7% nickel, .2% molybdenum 46XX

3.5% nickel, .25% molybdenum 48XX 1% chromium steels 51XX 1% chromium, 1.00% carbon 51XXX

1.5% chromium steels 52XX

1.5% chromium, 1.00% carbon 52XXX 1% chromium steel with .15% vanadium 61XX .5% chromium, .5% nickel, .20% molybdenum 86XX .5% chromium, .5% nickel, .25% molybdenum 87XX 2% silicon steels, .85% manganese 92XX

3.25% nickel, 1.20% chromium, .12% molybdenum 93XX Page 4-2 Par 4-2