(1) To prevent or minimize disassem bly, or reassembly.
(2) Resizing worn components (plate to size).
(3) Filling in damaged or corroded ar eas.
(4) To plate small areas of extremely large parts.
(5) To plate electrical contacts.
(6) To plate parts too large for existing baths.
(7) To supplement conventional plating.
(8) To plate components which become contaminated if immersed in a plating bath.
(9) To cadmium-plate ultrahigh strength steels without hydrogen embrittlement.
(10) On-site plating.
(11) Reverse current applications (e.g., stain removal, deburring, etching, and dynamic balancing).
b. Specifications. Selective plating (electrodepositions), when properly applied, will meet the following specifications and standards.
(1) QQ-C-320, Chromium Plating.
(2) QQ-N-290, Nickel Plating.
(3) QQ-P-416, Cadmium Plating.
(4) QQ-S-365, Silver Plating.
(5) QQ-Z-325, Zinc Plating.
(6) MIL-T-10727, Tin Plating.
(7) MIL-C-14550, Copper Plating.
(8) MIL-G-45204, Gold Plating.
c. General Requirements.
(1) Areas to be repaired by this process should be limited to small areas of large parts, particularly electrical or electronic parts.
(2) All solutions should be kept clean and free from contamination. Care should be taken to insure that the solutions are not con taminated by used anodes or other plating so lutions. Brush-plating solutions are not de signed to remove large amounts of scale, oil, or grease. Mechanical or chemical methods should be used to remove large amounts of scale or oxide. Use solvents to remove grease or oil.
(3) Brush-plating solutions are five to fifty times as concentrated as tank solutions.
The current densities used range from 500 to 4,000 amps/feet2. The voltages listed on the solution bottles have been precalculated to give proper current densities. Too high a cur rent density burns the plating, while too low a current density produces stressed deposits and low efficiencies. Agitation is provided by an ode/cathode motion. Too fast a motion results in low efficiencies and stressed deposits, and too slow a motion causes burning. A dry tool results in burnt plate, coarse grain structure, and unsound deposits. The tool cannot be too wet. Solution temperatures of 110 °F to 120 °F are reached during operation.
(4) Materials such as stainless steel, aluminum, chromium, and nickel (which have a passive surface) will require an activating operation to remove the passive surface. Dur ing the activating process, do not use solutions Par 4-62 Page 4-47
that have been previously used with reverse current (because of solution contamination).
d. Equipment. The power source should operate on either 110 or 220-volt alternating current (AC), 60 Hertz, single-phase input. It should have a capability to produce direct cur rent (DC) having smooth characteristics with controlled ripple and be able to output a cur rent of at least 25 amperes at 0 to 25 volts.
Minimum instrumentation of the power source should include a voltmeter, ammeter, and ampere-hour meter.
(1) The ammeter should provide a fullscale reading equal to the maximum capacity of the power source, and with an accuracy of ±5 percent of the current being measured.
(2) The voltmeter should have sufficient capacity to provide a full-scale reading equal to the maximum capacity of the power source and an accuracy of ±1.0 volt.
(3) An ampere-hour meter should be readable to 0.001 ampere-hour and have an ac curacy of ±0.01 ampere-hour.
(4) The stylus should be designed for rapid cooling and to hold anodes of various sizes and configurations. For safety, the anode holder should be insulated.
(5) The containers for holding and catching runoff solutions should be designed to the proper configuration and be inert to the specific solution.
(6) The mechanical cleaning equipment and materials should be designed and selected to prevent contamination of the parts to be cleaned.
e. Materials. The anodes should be of high-purity dense graphite or platinum-iridium alloys. Do not mix solutions from different suppliers. This could result in contamination.
f. Detail Requirements. On large parts, no area greater than approximately 10 percent of the total area of the part should be plated by this selective plating process. Small parts may be partially or completely plated. Special cases exceeding these limitations should be coordinated with the manufacturer of the plat ing equipment being used and their recom mendations should be followed.
g. Anode Selection. As a general guide, the contact area of the anode should be ap proximately one-third the size of the area to be plated. When selecting the anode, the configu ration of the part will dictate the shape of the anode.
h. Required Ampere-Hour Calculation.
The selected plating solution has a factor which is equal to the ampere-hours required to deposit 0.0001 inch on 1 square inch of sur face. Determine the thickness of plating de sired on a certain area, and multiply the solu tion factor times the plating thickness times the area in square inches to determine the am pere-hours required. This factor may vary be cause of temperature, current density, etc.
i. Cleaning. Remove corrosion, scale, oxide, and unacceptable plating prior to proc essing. Use a suitable solvent or cleaner to remove grease or oil.
j. Plating on Aluminum and Aluminum Base Alloys.
(1) Electroclean the area using direct current until water does not break on the sur face. This electroclean process should be ac complished at 10 to 15 volts, using the appro priate electroclean solution.
Page 4-48 Par 4-62
(2) Rinse the area in cold, clean tap water.
(3) Activate the area with reverse cur rent, 7 to 10 volts, in conjunction with the proper activating solution until a uniform, gray-to-black surface is obtained.
(4) Rinse thoroughly in cold, clean tap water.
(5) Immediately electroplate to color while the area is still wet, using the appropriate nickel solution.
(6) Rinse thoroughly.
(7) Immediately continue plating with any other solution to desired thickness.
(8) Rinse and dry.
k. Plating on Copper and Copper Base Alloys.
(1) Electroclean the area using direct current until water does not break on the sur face. The electroclean process should be ac complished at 8 to 12 volts using the appropri ate electroclean solution.
(2) Rinse the area in cold, clean tap water.
(3) Immediately electroplate the area with any of the plating solutions, except silver.
Silver requires an undercoat.
(4) Rinse and dry.
l. Plating on 300 and 400 Series Stain less Steels, Nickel Base Alloys, Chrome Base Alloys, High Nickel Ferrous Alloys, Cobalt Base Alloys, Nickel Plate, and Chrome Plate.
(1) Electroclean the area using direct current until water does not break on the sur face. This electroclean process should be ac complished at 12 to 20 volts using the appro priate electrocleaning solution.
(2) Rinse the area in cold, clean tap water.
(3) Activate the surface using direct current for 1 to 2 minutes, using the activating solution, and accomplish at 6 to 20 volts.
(4) Do not rinse.
(5) Immediately nickel-flash the surface to a thickness of 0.00005 to 0.0001 inch, using the appropriate nickel solution.
(6) Rinse thoroughly.
(7) Immediately continue plating with any other solution to desired thickness.
(8) Rinse and dry.
m. Plating on Low-Carbon Steels (Heat Treated to 180,000 psi).
(1) Electroclean the area using direct current until water does not break on the sur face. This electroclean process should be ac complished at 12 to 20 volts, using the appro priate electrocleaning solution.
(2) Rinse the area in cold, clean tap water.
(3) Reverse-current etch at 8 to 10 volts, using the appropriate activating solu tion, until a uniform gray surface is obtained.
(4) Rinse thoroughly.
Par 4-62 Page 4-49
(5) Immediately electroplate the part using any solutions, except copper or silver.
Both of these require undercoats.
(6) Rinse and dry.
n. Plating on Cast Iron and High-Carbon Steels (Steels Heat Treated to 180,000 psi).
(1) Electroclean the area using direct current until water does not break on the sur face. This electroclean process should be ac complished at 12 to 20 volts, using the appro priate electrocleaning solution.
(2) Rinse the area thoroughly in cold, clean tap water.
(3) Reverse-current etch at 8 to 10 volts, using the appropriate etching solu tion, until a uniform gray is obtained.
(4) Rinse thoroughly.
(5) Remove surface smut with 15 to 25 volts using the appropriate activating solu tion.
(6) Rinse thoroughly.
(7) Electroplate immediately, using any of the solutions, except copper or silver (both of these require undercoats).
(8) Rinse and dry.
o. Plating on Ultrahigh Strength Steels (Heat Treated Above 180,000 psi).
(1) Electroclean the area using reverse current until water does not break on the sur face. This electroclean process should be ac complished at 8 to 12 volts using the appropri ate electroclean solution.
(2) Rinse the area thoroughly in cold, clean tap water.
(3) Immediately electroplate the part, using either nickel, chromium, gold, or cad mium. Other metals require an undercoat of one of the above. Plate initially at the highest voltage recommended for the solution so as to develop an initial barrier layer. Then reduce to standard voltage.
(4) Rinse and dry.
(5) Bake the part for 4 hours at 375 °F ± 25 °F.
NOTE: Where the solution vendor provides substantiating data that hy drogen embrittlement will not result from plating with a particular solu tion, then a postbake is not required.
This substantiating data can be in the form of aircraft industry manufac turer’s process specifications, military specifications, or other suitable data.
NOTE: Acid etching should be avoided, if possible. Where etching is absolutely necessary, it should always be done with reverse current. Use al kaline solutions for initial deposits.
p. Dissimilar Metals and Changing Base. As a general rule, when plating two dis similar metals, follow the plating procedure for the one with the most steps or activation. If activating steps have to be mixed, use reversecurrent activation steps prior to direct-current activation steps.
q. Plating Solution Selection.
(1) Alkaline and neutral solutions are to be used on porous base metals, white metals, high-strength steel, and for improved coating Page 4-50 Par 4-62
ability. Acid solutions are to be used for rapid buildup and as a laminating structure material in conjunction with alkaline-type solutions.
(2) Chrome brush-plating solutions do not yield as hard a deposit as bath-plating so lutions. The hardness is about 600 Brinell as compared to 1,000 Brinell for hard chrome de posited from a tank.
(3) Silver-immersion deposits will form with no current flowing on most base metals from the silver brush-plating solutions. Such deposits have poor adhesion to the base metal.
Consequently, a flash of a more noble metal should be deposited prior to silver plating to develop a good bond.
(4) In general, brush plating gives less hydrogen embrittlement and a lower fatigue strength loss than does equivalent tank depos its. However, all brush-plated, ultrahigh strength steel parts (heat treated above 180,000 psi) should be baked, as mentioned, unless it is specifically known that embrittle ment is not a factor.
r. Qualification Tests. All brush-plated surfaces should be tested for adhesion of the electrodeposit. Apply a 1-inch wide strip of Minnesota Mining and Manufacturing tape code 250, or an approved equal, with the adhe sive side to the freshly plated surface. Apply the tape with heavy hand pressure and remove it with one quick motion perpendicular to the plated surface. Any plating adhering to the tape should be cause for rejection.
s. Personnel Training for Quality Con trol. Manufacturers of selective-plating equipment provide training in application techniques at their facilities. Personnel per forming selective plating must have adequate knowledge of the methods, techniques, and practices involved. These personnel should be certified as qualified operators by the manu facturers of the products used.
4-63. 4-73. [RESERVED.] Par 4-62 Page 4-51 (and 4-52)
SECTION 5. WELDING AND BRAZING
4-74. GENERAL. This section covers weld repairs to aircraft and component parts only.
Observe the following procedures when using such equipment as gas tungsten arc welding (GTAW), gas metal arc welding (GMAW), plasma arc welding, and oxyacetylene gas welding. When repairs of any of these flight-critical parts are required, it is extremely important to make the weld repairs equal to the original weld. Identifying the kind of metal to be welded, identifying the kind of welding pro cess used in building the part originally, and determining the best way to make welded re pairs are of utmost importance.
a. Welding is one of the three commonly used methods of joining metals without the use of fasteners. Welding is done by melting the edges of two pieces of metal to be joined and allowing the molten material to flow together so the two pieces will become one.
b. Brazing is similar to welding in that heat is used to join the material; but rather than melting, the metal is heated only enough to melt a brazing rod having a much lower melt ing point. When this brazing rod melts, it wets the surfaces to be joined, and when it cools and solidifies, it bonds the pieces together.
c. Soldering is similar to brazing except that brazing materials normally melt at tempera tures above 425 °C (800 °F), while solders melt at temperatures considerably lower.
d. The next step in making airworthy weld repairs is to decide the best process to use, considering the available state-of-the-art welding equipment, and then deciding the cor rect weld-filler material to use. Before any weld repairs can be made, the metal parts to be welded must be cleaned properly, fitted and jigged properly, and all defective welds must be removed to prepare for an aircraft quality weld repair.
e. Finally, after the weld is completed, the weld must be inspected for defects. All these things are necessary in order to make an air worthy weld repair.
f. Aircraft welding Qualifications. Four groups of metals a person can be certified and qualified to use are:
(1) Group 1, 4130 Steel.
(2) Group 2, Stainless Steel.
(3) Group 3, Aluminum
(4) Group 4, Titanium.
g. For other group listing of metal the welder may qualify, refer to Mil-Std-1595A.
h. Most large business or agencies conduct their own certification tests, or they have an outside testing lab validate the certification tests.
4-75. EQUIPMENT SELECTION. Use the welding equipment manufacturer’s infor mation to determine if the equipment will sat isfy the requirements for the type of welding operation being undertaken. Disregarding such detailed operating instructions may cause substandard welds. For example, when using GTAW equipment, a weld can be contami nated with tungsten if the proper size electrode is not used when welding with direct current reverse polarity. Another example, the deple tion of the inert gas supply below the critical level causes a reduction in the gas flow and will increase the danger of atmospheric con tamination.
(a) Electric welding equipment versatility requires careful selection of the type current and polarity to b used. Since the composition and thickness of metals are deciding Par 4-74 Page 4-53
factors, the selection may vary with each spe cific application. Metals having refractory sur face oxide films (i.e., magnesium alloys and aluminum and its alloys), are generally welded with alternating current (AC), while direct cur rent (DC) is used for carbon, low alloy, noncorrodible, and heat-resisting steels. General recommendations covering current and polar ity are shown in table 4-12.
(b) Oxyacetylene gas equipment is suitable for welding most metals. It is not, however, the best method to use on such materials as stainless steel, magnesium, and aluminum al loys; because of base metal oxidization, dis tortion, and loss of ductility.
NOTE: If oxyacetylene is used for welding stainless steel or aluminum, all flux must be removed, as it may cause corrosion.
4-76. ACCURATELY IDENTIFY THE TYPE OF MATERIAL TO BE RE PAIRED. If positive identification of the material is not possible, contact the aircraft manufacturer or subject the item to a metallur gical laboratory analysis. Before any welding is attempted, carefully consider the weldability of the alloy, since all alloys are not readily weldable. The following steels are readily weldable; plain carbon (of the 1000 series), nickel steel (of the Society of Automotive En gineers (SAE) 2300 series), chrome-nickel al loys (of the SAE 3100 series), chromemolybdenum steels (of the SAE 4100 series), and low nickel-chrome-molybdenum steel (of the SAE 8600 series).
4-77. PREPARATION FOR WELDING.
a. Hold elements to be welded in a welding jig or fixture which is sufficiently rigid to pre vent misalignment due to expansion and con traction of the heated material and which positively and accurately positions the pieces to be welded.
b. Clean parts to be welded with a wire brush or other suitable method prior to weld ing. Do not use a brush of dissimilar metal, such as brass or bronze on steel. The small deposit left by a brass or bronze brush will materially weaken the weld, and may cause cracking or subsequent failure of the weld. If the members are metallized, the surface metal may be removed by careful sandblasting fol lowed by a light buffing with emery cloth.
4-78. INSPECTION OF A COMPLETED WELD. Visually inspect the completed weld for the following:
(a) The weld has a smooth seam and uniform thickness. Visual inspection shall be made of the completed weld to check for undercut and/or smooth blending of the weld contour into the base metal.
(b) The weld is tapered smoothly into the base metal.
(c) No oxide has formed on the base metal more than 1/2 inch from the weld.
(d) There are no signs of blowholes, poros ity, or projecting globules. Many military specifications, as well as American Society of Testing Materials (ASTM) codes, specify ac ceptable limits of porosity and other types of defects that are acceptable.
(e) The base metal shows no signs of pitting, burning, cracking, or distortion.
(f) The depth of penetration insures fusion of base metal and filler rod.
(g) The welding scale is removed. The welding scale can be removed using a wire brush or by sandblasting. Remove any Page 4-54 Par 4-75
roll over, cold lab, or unfued weld metal.
Check underside of welded joint for defects.
TABLE 4-12. Current and polarity selection for inert gas welding.
MATERIAL
ALTERNATING
CURRENT DIRECT
CURRENT With High- Frequency Stabilization
STRAIGHT Polarity Magnesium up to ¹/8 in. thick.................................................. 1 N.R.
Magnesium above ³/16 in. thick............................................... 1 N.R.
Magnesium Castings................................................................ 1 N.R.
Aluminum up to ³/32 in. thick.................................................. 1 N.R.
Aluminum over ³/32 in. thick ................................................... 1 N.R.
Aluminum Castings ................................................................. 1 N.R.
Stainless Steel1
Low Carbon Steel, 0.015 to 0.030 in1
Low Carbon Steel, 0.030 to 0.125 in. ..................................... N.R. 1 1 Recommended N.R. Not Recommended
4-79. MICROFISSURES Cracks in parts and materials can vary from tiny microfissures, that are visible only with magnification, to those easily identified by unaided eyes. Microfissures are the worst type of defect for two reasons; they are often hard to detect, and they produce the worst form of notch effect/stress concentration. Once they form, they propagate with repeated applications of stress and lead to early failures. Every possible means should be used to detect the presence of cracks, and en sure their complete removal before welding operations proceed. (See figure 4-26.)
4-80. NONDESTRUCTIVE TESTING or evaluation is advisable in critical applications.
Nondestructive testing methods such as; mag netic particle, liquid penetrant, radiography, ultrasonic, eddy current, and acoustic emission can be used; however, they require trained and qualified people to apply them.
4-81. PRACTICES TO GUARD AGAINST Do not file or grind welds in an effort to create a smooth appearance, as such treatment causes a loss of strength. Do not fill welds with solder, brazing metal, or any other filler. When it is necessary to weld a FIGURE 4-26. Common defects to avoid when fitting and welding aircraft certification cluster.
joint which was previously welded, remove all of the old weld material before rewelding.
Avoid welding over a weld, because reheating may cause the material to lose its strength and become brittle. Never weld a joint which has been previously brazed.
4-82. TORCH SIZE (Oxyacetylene weld ing). When using oxyacetylene welding, the torch tip size depends upon the thickness of the material to be welded. Commonly used Par 4-78 Page 4-55
sizes, proven satisfactory by experience, are shown in table 4-13.
TABLE 4-13. Torch tip sizes.
Thickness of steel Diameter of Drill size (in inches) hole in tip
0.015 to 0.031 0.026 71
0.031 to 0.065 .031 68
0.065 to 0.125 .037 63
0.125 to 0.188 .042 58
0.188 to 0.250 .055 54
0.250 to 0.375 .067 51
4-83. WELDING RODS AND ELEC TRODES Use welding rods and electrodes that are compatible with the materials to be welded. Welding rods and electrodes for vari ous applications have special properties suit able for the application intended.
Lap welds are used in shear applications. The weld throat of the fillet weld is considered the plane 45 degrees to the surface plane of the sheet being welded and is equal to 0.707 times the thickness of the sheet stock. (See fig ure 4-27.)
PWS = 0.707xtx1xFwsu where: PWS = the allowable tensile strength of the joint.
t = the thickness of the sheet stock (the throat of the weld joint.
l = the length of the weld joint.
Fwsu= the shear strength of the filled rod material.
FIGURE 4-27. Lap Weld Strength Calculation
4-84. ROSETTE WELDS are generally employed to fuse an inner reinforcing tube (liner) with the outer member. Where a rosette weld is used, drill a hole, (in the outside tube only) of sufficient size to insure fusion of the inner tube. A hole diameter of approximately one-fourth the tube diameter of the outer tube serves adequately for this purpose. In cases of tight-fitting sleeves or inner liners, the rosettes may be omitted. Rosette weld edge distance is 1/2 the diameter of the tube, as measured from the edge of the rosette hole to the end of the inside and outside tube. Rosettes shall not be considered when determining the strength of a welded form. Drill an 1/8-inch hole in the lower tube in the center of the intended rosette weld so the heat does not burn away the outer tube. This small hole tends to bleed off the heat from the torch and keeps the size of the rosette small.
4-85. HEAT-TREATED MEMBERS Certain structural parts may be heat treated and, therefore, could require special handling.
In general, the more responsive an alloy steel is to heat treatment, the less suitable it is for welding because of its tendency to become brittle and lose its ductility in the welded area.
Weld the members which depend on heat treatment for their original physical properties by using a welding rod suitable for producing heat-treated values comparable to those of the original members. (See paragraph 4-74.) Af ter welding, heat treat the affected members to the manufacturer’s specifications.
4-86. TYPES OF WELDING.
a. Gas Welding. A fuel gas such as acety lene or hydrogen is mixed inside a welding torch with oxygen to produce a flame with a temperature of around 6,300 °F (3,482 ºC).
Page 4-56 Par 4-75
This flame is used to melt the materials to be welded. A filler rod is melted into the puddle of molten metal to reinforce the weld. When highly-reactive metals such as aluminum are gas welded, they must be covered with flux to exclude oxygen from the molten metal and keep oxides from forming which would de crease the strength of the weld. (An illustration of a carburizing flame, a neutral flame, and an oxidizing flame is shown in figure 4-28.)
b. Shielded Metal Arc Welding (SMAW).
This method is the most familiar and common type and is known in the trade as stick weld ing. A metal wire rod coated with a welding flux is clamped in an electrode holder con nected to the power supply with a heavy elec trical cable. The metal to be welded is also attached to the power supply. The electrical power is supplied to the work at a low voltage FIGURE 4-28. Basic gas-welding flames: Each has dis tinctive shape, color and sound. Neutral flame is the most used.
and high current and may be either AC or DC, depending upon the type of welding being done. An arc is struck between the rod and the work and produces heat in excess of 10,000 °F, which melts both the material and the rod. As the flux melts, it releases an inert gas which shields the molten puddle from oxygen in the air and prevents oxidation. The molten flux covers the weld and hardens to an airtight slag cover that protects the weld bead as it cools. This slag must be chipped off to examine the weld.
c. Gas Metal Arc Welding (GMAW). This method of welding was formerly called Metal Inert Gas (MIG) welding and is an improve ment over stick welding because an uncoated wire electrode is fed into the torch and an inert gas such as argon, helium, or carbon dioxide flows out around the wire to protect the puddle from oxygen. The power supply connects between the torch and the work, and the arc produces the intense heat needed to melt the work and the electrode. Low-voltage highcurrent DC is used almost exclusively with GMAW welding. GMAW is used more for large-volume production work than for aircraft repair.
d. Gas Tungsten Arc Welding (GTAW).
This is the form of electric arc welding that fills most of the needs in aircraft maintenance.
It is more commonly known as Tungsten Inert Gas (TIG) welding and by the trade names of Heliarc or Heliweld. These trade names were derived from the fact that the inert gas origi nally used was helium.
(1) Rather than using a consumable electrode such as is used in both of the other two meth ods we have discussed, the electrode in TIG welding is a tungsten rod. (In earlier proce dures using this form of welding, a carbon electrode was used, but it has been replaced almost exclusively with tungsten.)
Par 4-86 Page 4-57
(2) The 250+ amp arc between the electrode and the work melts the metal at 5,432 ºF, and a filler rod is manually fed into the molten puddle. A stream of inert gas such as argon or helium flows out of the torch and envelopes the arc, thereby preventing the formation of oxides in the puddle.
(3) The versatility of TIG welding is in creased by the power supply that is used. Di rect current of either polarity or alternating current may be used. (See figures 4-29 and 4-30.)
FIGURE 4-29. Set TIG welder to DC current, straight polarity for welding mild steel, stainless steel and ti tanium FIGURE 4-30. Set TIG to AC current for welding aluminum and magnesium.
4-87. ELECTRIC-RESISTANCE WELD ING. Many thin sheet metal parts for aircraft, especially stainless steel parts, are joined by one of the forms of electric resistance welding, either spot welding or seam welding.
a. Spot Welding. Two copper electrodes are held in the jaws of the spot welding machine, and the material to be welded is clamped be tween them. Pressure is applied to hold the electrodes tightly together, and electrical cur rent flows through the electrodes and the mate rial. The resistance of the material being welded is so much higher than that of the cop per electrodes that enough heat is generated to melt the metal. The pressure on the electrodes forces the molten spots in the two pieces of metal to unite, and this pressure is held after the current stops flowing long enough for the metal to solidify. Refer to MIL HDBK-5 for joint construction and strength data. The amount of current, pressure, and dwell time are all carefully controlled and matched to the type of material and the thickness to produce the cor rect spot welds. (See figure 4-31.)
b. Seam Welding. Rather than having to release the electrodes and move the material to form a series of overlapping spot welds, a seam-welding machine is used to manufacture FIGURE 4-31. In spot welding, heat is produced by electrical resistance between copper electrodes. Pres sure is simultaneously applied to electrode tips to force metal together to complete fusing process. Spot-weld nugget size is directly related to tip size.
fuel tanks and other components where a con tinuous weld is needed. Two copper wheels Page 4-58 Par 4-86
replace the bar-shaped electrodes. The metal to be welded is moved between them, and electric pulses create spots of molten metal that overlap to form the continuous seam.
4-88. BRAZING. Brazing refers to a group of metal-joining processes in which the bond ing material is a nonferrous metal or alloy with a melting point higher than 425 C (800 F), but lower than that of the metals being joined.
Brazing includes silver brazing (erroneously called silver soldering or hard soldering), cop per brazing, and aluminum brazing.
NOTE: Never weld over a previously brazed joint.
a. Brazing requires less heat than welding and can be used to join metals that are dam aged by high heat. However, because the strength of brazed joints is not as great as welded joints, brazing is not used for structural repairs on aircraft. In deciding whether braz ing of a joint is justified, it should be remem bered that a metal, which will be subjected to a sustained high temperature in use, should not be brazed.
b. A brazing flux is necessary to obtain a good union between the clean base metal and the filler metal. There are a number of readily available manufactured fluxes conforming to AWS and AMT specifications.
c. The base metal should be preheated slowly with a mild flame. When it reaches a dull-red heat (in the case of steel), the rod should be heated to a dark (or purple) color and dipped into the flux. Since enough flux adheres to the rod, it is not necessary to spread it over the surface of the metal.
d. A neutral flame is used in most brazing applications. However, a slightly oxidizing flame should be used when copper-zinc, copper-zinc-silicon, or copper-zinc-nickel-silicon filler alloys are used. When brazing aluminum and its alloys, a neutral flame is preferred, but if difficulties are encountered, a slightly re duced flame is preferred to an oxidizing flame.
e. The filler rod can now be brought near the tip of the torch, causing the molten bronze to flow over a small area of the seam. The base metal must be at the flowing temperature of the filler metal before it will flow into the joint. The brazing metal melts when applied to the steel and runs into the joint by capillary at traction. In braze welding, the rod should continue to be added, as the brazing pro gresses, with a rhythmic dipping action; so that the bead will be built to a uniform width and height. The job should be completed rapidly and with as few passes of the rod and torch as possible.
f. When the job is finished, the metal should be allowed to cool slowly. After cool ing, remove the flux from the parts by im mersing them for 30 minutes in a lye solution.
(1) Copper brazing of steel is normally done in a special furnace having a controlled atmos phere, and at a temperature so high that field repairs are seldom feasible. If copper brazing is attempted without a controlled atmosphere, the copper will probably not completely wet and fill the joint. Therefore, c opper brazing in any conditions other than appropriately con trolled conditions is not recommended.
(a) The allowable shear strength for copper brazing of steel alloys should be 15 thousand pounds per square inch (kpsi), for all condi tions of heat treatment.
(b) The effect of the brazing process on the strength of the parent or base metal of steel alloys should be considered in the structural design. Where copper furnace brazing is em ployed, the calculated allowable strength of Par 4-87 Page 4-59