tour of the joint to the plate. In this operation formed by any two adjacent fingers of the avoid unnecessary heating, and exercise care to plate. After the plate is formed and tack prevent damage at the point of the angle welded to the cluster joint, weld all the plate edges to the cluster joint.
TABLE 4-15. Chart showing Welding Filler Rod selection.
Welding Rod # AMS Spec. AWS Spec. Welds these Metals 4130 4140 4043 308L 316L AZ61A ERTi-5 AMS 6457 AMS 6452 AMS 4190 AMS 5692 AMS 5692 AMS 4350 AMS 4954 AWS A5.18 AWS A5.28 AWS A5.10 AWS A5.9 AWS A5.9 AWS A5.19 AWS A5-16 Mild Steel, 4130 steel 4140 Steel Most weldable Aluminum 304 Stainless steel 316 Stainless steel AZ61A Magnesium Titanium Par 4-91 Page 4-63
LONGERON DENTED AT A STATION.
THICKNESS OF PATCH PLATE
SAME AS LONGERON THICKNESS.
PATCH PLATE BEFORE FORMING AND WELDING.
PATCH PLATE FORMED AND WELDED TO TUBES.
FIGURE 4-34. Finger patch repairs for members dented at a cluster.
Page 4-64 Par 4-91
d. Members Dented in a Bay. R e p a i r dented, bent, cracked, or otherwise damaged tubular members by using a split-sleeve rein forcement. Carefully straighten the damaged member, and in the case of cracks, drill No. 40 (0.098) inch stop holes at the ends of the crack.
4-92. REPAIR BY WELDED SLEEVE.
This repair is outlined in figure 4-35. Select a length of steel tube sleeve having an inside di ameter approximately equal to the outside di ameter of the damaged tube and of the same material, and at least the same wall thickness.
Diagonally cut the sleeve reinforcement at a 30-degree angle on both ends so that the minimum distance of the sleeve from the edge of the crack or dent is not less than 1-1/2 times the diameter of the damaged tube. Cut through the entire length of the reinforcement sleeve, and separate the half-sections of the sleeve.
Clamp the two sleeve sections to the proper positions on the affected areas of the original tube. Weld the reinforcement sleeve along the length of the two sides, and weld both ends of the sleeve to the damaged tube. (See fig ure 4-35.) The filling of dents or cracks with welding rod in lieu of reinforcing the member is not acceptable.
4-93. REPAIR BY BOLTED SLEEVE.
Do not use bolted-sleeve repairs on welded steel-tube structure unless specifically author ized by the manufacturer or the FAA. The tube area removed by the bolt holes, in this type of repair, may prove critical.
4-94. WELDED-PATCH REPAIR. Dents or holes in tubing may be repaired by using a patch of the same material, one gauge thicker.
(See figure 4-36.)
a. Dented Tubing.
(1) Dents are not deeper than 1/10 of tube diameter, do not involve more than 1/4 of the tube circumference, and are not longer than tube diameter.
(2) Dents are free from cracks, abrasions, and sharp corners.
(3) The dented tubing can be substantially re formed, without cracking, before application of the patch.
b. Punctured Tubing. Holes are not longer than tube diameter and involve not more than 1/4 of tube circumference.
4-95. SPLICING TUBING BY INNER SLEEVE METHOD. If the damage to a structural tube is such that a partial replace ment of the tube is necessary, the inner-sleeve splice is recommended; especially where a smooth tube surface is desired. (See fig ure 4-37.)
a. Make a diagonal cut when removing the damaged portion of the tube, and remove the burr from the edges of the cut by filing or similar means. Diagonally cut a replacement steel tube of the same material and diameter, and at least the same wall thickness, to match the length of the removed portion of the dam aged tube. At each end of the replacement tube allow a 1/8-inch gap from the diagonal cuts to the stubs of the original tube. Select a length of steel tubing of the same material, and at least the same wall thickness, and of an out side diameter equal to the inside diameter of the damaged tube. Fit this inner-sleeve tube material snugly within the original tube, with a maximum diameter difference of 1/16 inch.
From this inner-sleeve tube material cut two sections of tubing, each of such a length that the ends of the inner sleeve will be a minimum distance of 1-1/2-tube diameters from the nearest end of the diagonal cut.
Par 4-91 Page 4-65
DENTED OR BENT TUBE
CRACKED TUBE
- REINFORCEMENT TUBE SPLIT NOTE:
LOCALLY DENTED OR
BENT MEMBERS SHOULD
FIRST BE REFORMED IN CLAMP.
REINFORCEMENT SLEEVE TO BE OF SAME
MATERIAL AND AT LEAST THE SAME GAUGE AS TUBE BEING REPAIRED.
1-1/2 A WELD 1-1/2 A
AS ALTERNATIVE TO SPLIT TUBE,
A TWO-PIECE REINFORCEMENT
SLEEVE MAY BE FORMED FROM STEEL SHEET OF THE SAME MATERIAL 30° AND AT LEAST THE SAME GAUGE AS - 1A → 1A - THE DAMAGED TUBE. USE FISHMOUTH +1-1/2A• 91-112
ENDS AND FOUR ROSETTE WELDS AS SHOWN.
FIGURE 4-35. Members dented in a bay (repairs by welded sleeve).
Page 4-66 Par 4-95
FIGURE 4-36. Welded patch repair.
b. If the inner sleeve fits very tightly in the replacement tube, chill the sleeve with dry ice or cold water. If this is insufficient, polish down the diameter of the sleeve with emery cloth. Tack the outer and inner replacement tubes using rosette welds. Weld the inner sleeve to the tube stubs through the 1/8-inch gap, forming a weld bead over the gap.
4-96. SPLICING TUBING BY OUTER SLEEVE METHOD. If partial replacement of a tube is necessary, make the outer-sleeve splice using a replacement tube of the same di ameter. Since the outer-sleeve splice requires the greatest amount of welding, it should be used only when the other splicing methods are not suitable. Information on the replacement by use of the outer-sleeve method is given in figure 4-38 and figure 4-39.
a. Remove the damaged section of a tube utilizing a 90-degree cut. Cut a replacement steel tube of the same material, diameter, and at least the same wall thickness to match the length of the removed portion of the damaged tube. This replacement tube must bear against the stubs of the original tube with a total toler ance not to exceed 1/32 inch. The outer-sleeve tube material selected must be of the same material and at least the same wall thickness as the original tube. The clearance between inside diameter of the sleeve and the outside diameter of the original tube may not exceed 1/16 inch.
b. From this outer-sleeve tube material, cut diagonally (or fishmouth) two sections of tub ing, each of such length that the nearest end of the outer sleeve is a minimum distance of 1-1/2-tube diameters from the end of the cut on the original tube. Use a fishmouth sleeve wherever possible. Deburr the edges of the sleeves, replacement tube, and the original tube stubs.
c. Slip the two sleeves over the replacement tube, align the replacement tube with the origi nal tube stubs, and slip the sleeves over the center of each joint. Adjust the sleeves to suit the area and provide maximum reinforcement.
d. Tack weld the two sleeves to the re placement tube in two places before welding.
Apply a uniform weld around both ends of one of the reinforcement sleeves and allow the weld to cool; then, weld around both ends of the remaining reinforcement tube. Allow one sleeve weld to cool before welding the re maining tube to prevent undue warping.
Par 4-95 Page 4-67
FIGURE 4-37. Splicing by inner-sleeve method.
4-97. SPLICING USING LARGER DI AMETER REPLACEMENT TUBES. The method of splicing structural tubes, as shown in figure 4-40, requires the least amount of cutting and welding. However, this splicing method cannot be used where the damaged tube is cut too near the adjacent cluster joints, or where bracket-mounting provisions make it necessary to maintain the same replacement tube diameter as the original. As an aid to in stalling the replacement tube, squarely cut the original damaged tube leaving a minimum short stub equal to 2-1/2-tube diameters on one end and a minimum long stub equal to 4-1/2-tube diameters on the other end. Select a length of steel tube of the same material and at least the same wall thickness, having an inside diameter approximately equal to the outside diameter of the damaged tube. Fit this re placement tube material snugly around the original tube with a maximum diameter differ ence of 1/16 inch. From this replacement tube material, cut a section of tubing diagonally (or fishmouth) of such a length that each end of the tube is a minimum distance of 1-1/2-tube diameters from the end of the cut on the origi nal tube. Use a fishmouth cut replacement tube wherever possible. Deburr the edges of the replacement tube and original tube stubs.
If a fishmouth cut is used, file out the sharp ra dius of the cut with a small round file.
Page 4-68 Par 4-97
30° SLEEVE 112-112- 30 A
ROSETTE WELDS MAY - WELD
BE OMITTED WHEN SLEEVES FIT TIGHTLY.
- REPLAGEMENT TUBE
ORIGINAL TUBE , FISH-MOUTH 1/2A- SLEEVE
- 1/2A 1/4A == = -A-
ROSETTE WELDS MAY WELD
BE OMITTED WHEN SLEEVES FIT TIGHTLY.
REPLACEMENT TUBE
ORIGINAL TUBE FOUR ROSETTE •WELD HERE FIRST ORIGINAL TUBE WELDS +1/4A
- 1/8" GAP +-1½A 7/24 1½A* FOR WELDING ALTERNATIVE SPLIT SLEEVE SPLICE ~ IF OUTSIDE DIAMETER OF ORIGINAL TUBE IS LESS THAN 1 INCH, SPLIT SLEEVE MAY BE MADE FROM STEEL TUBE OR SHEET STEEL. USE SAME MATERIAL OF AT LEAST THE SAME GAUGE.
FIGURE 4-38. Splicing by outer-sleeve method (replacement by welded outside sleeve).
Par 4-97 Page 4-69
‹ ORIGINAL TUBE
SLEEVE SLEEVE TUBE +CY TUBE ń/4C 1/2B
ROSETTE ORIGINAL TUBE WELD WELD 1/4A LA- 30° 30 ORIGINAL TUBE 1/2A~ 112 SLEEVE HE GAP REPLACEMENT TUBE SLEEVE TUBE
TUBE BETWEEN SLEEVES FOR WELDING.
FIGURE 4-39. Tube replacement at a station by welded outer sleeves.
-2-1/2A REPLACEMENT TUBE 30° 30 ORIGINAL → 112A TUBE +1-1/2A→
- REPLACEMENT TUBE na
- 4-1/2A 30 · →112A ORIGINAL TUBE
•1-112A→ FIGURE 4-40. Splicing using larger diameter replacement tube.
Page 4-70 Par 4-97
Spring the long stub of the original tube from the normal position, slip the replacement tube over the long stub, and then back over the short stub. Center the replacement tube be tween the stubs of the original tube. Tack weld one end of the replacement tube in sev eral places, then weld completely around the end. In order to prevent distortion, allow the weld to cool completely, then weld the re maining end of the replacement tube to the original tube.
4-98. REPAIRS AT BUILT-IN FUSE LAGE FITTINGS. Make splices in accor dance with the methods described in para graphs 4-86 through 4-92. Repair built-in fu selage fittings in the manner shown in fig ure 4-41. The following paragraphs outline the different methods as shown in figure 4-41.
a. Tube of Larger Diameter Than Origi nal. A tube (sleeve) of larger diameter than the original is used in the method shown in figure 4-41 (A). The forward splice is a 30-degree scarf splice. Cut the rear longeron (right) approximately 4 inches from the cen terline of the joint and fit a 1 inch long spacer over the longeron, and edge weld this spacer and longeron. Make a tapered “V” cut ap proximately 2 inches long in the aft end of the outer sleeve, and swage the end of the outer sleeve to fit the longeron and weld.
b. Tube of Same Diameter as Original. In the method shown in figure 4-41 (B) the new section is the same size as the longeron forward (left) of the fitting. The rear end (right) of the tube is cut at 30 degrees and forms the outside sleeve of the scarf splice. A sleeve is centered over the forward joint as in dicated.
c. Simple Sleeve. In figure 4-41 (C), it is as sumed the longeron is the same size on each side of the fitting. It is repaired by a sleeve of larger diameter than the longeron.
d. Large Difference in Longeron Diameter Each Side of Fitting. Figure 4-41 (D) as sumes that there is 1/4-inch difference in the diameter of the longeron on the two sides of the fitting. The section of longeron forward (left) of the fitting is cut at 30 degrees, and a section of tubing of the same size as the tube and of such length as to extend well to the rear (right) of the fitting is slipped through it. One end is cut at 30 degrees to fit the 30-degree scarf at left, and the other end fishmouthed.
This makes it possible to insert a tube of proper diameter to form an inside sleeve for the tube on the left of the fitting and an outside sleeve for the tube on the right of the fitting.
4-99. ENGINE-MOUNT REPAIRS. A l l welding on an engine mount must be of the highest quality, since vibration tends to ac centuate any minor defect. Engine-mount members should preferably be repaired by us ing a larger diameter replacement tube, tele scoped over the stub of the original member, and using fishmouth and rosette welds. How ever, 30-degree scarf welds in place of the fishmouth welds will be considered acceptable for engine-mount repair work.
a. Repaired engine mounts must be checked for accurate alignment. When tubes are used to replace bent or damaged ones, the original alignment of the structure must be maintained.
When drawings are not available, this can be done by measuring the distance between points of corresponding members that have not been distorted.
b. Grind out all cracked welds.
c. Use only high-grade metallurgically con trolled (mc) welding rods for engine-mount re pairs.
Par 4-97 Page 4-71
WELD SPACER APPROXIMATELY "A" LONG WELDED ON
INSIDE TUBE → 3A- (A) (B) GENERAL NOTE: -
ALL ROSETTE WELDS (C) TO BE & DIAMETER OF THE ORIGINAL TUBES.
GAP $"* 30° (D) FIGURE 4-41. Repairs at built-in fuselage fittings.
Page 4-72 Par 4-99
d. If all members are out of alignment, re ject the engine mount and replace with one supplied by the manufacturer or one which was built to conform to the manufacturer’s draw ings. The method of checking the alignment of the fuselage or nacelle points should be re quested from the manufacturer.
e. Repair minor damage, such as a crack adjacent to an engine-attachment lug, by rew elding the ring and extending a gusset or a mounting lug past the damaged area. Enginemount rings which are extensively damaged must not be repaired, unless the method of re pair is specifically approved by the FAA, or the repair is accomplished in accordance with FAA-approved instructions.
f. If the manufacturer stress relieved the engine mount after welding it, the engine mount should be re-stress relieved after the weld repairs are made.
4-100. BUILT-UP TUBULAR WING OR TAIL-SPARS. Repair built-up tubular wing or tail-spars by using any of the applicable splices and methods of repair shown in fig ure 4-35 through figure 4-45, provided the spars are not heat treated. In the case of heattreated spars, the entire spar assembly would have to be reheat treated to the manufacturer’s specifications after completion of the repair.
In general, this will be found less practicable than replacing the spar with one furnished by the manufacturer or holder of the PMA for the part.
4-101. WING-BRACE STRUTS AND TAIL-BRACE STRUTS. In general, it will be found advantageous to replace damaged wing-brace struts made either from rounded or streamlined tubing with new members pur chased from the original manufacturer. How ever, there is no objection, from an airworthi ness point of view, to repairing such members in a proper manner. An acceptable method of repair, if streamlined tubing is used, will be found in figure 4-43. Repair similar members made of round tubes using a standard splice, as shown in figure 4-35, figure 4-37, or fig ure 4-38.
a. Location of Splices. Steel-brace struts may be spliced at any point along the length of the strut provided the splice does not overlap part of an end fitting. The jury-strut attach ment is not considered an end fitting; there fore, a splice may be made at this point. The repair procedure and workmanship minimize distortion due to welding and the necessity for subsequent straightening operations. Observe every repaired strut carefully during initial flights to ascertain that the vibration charac teristics of the strut and attaching components are not adversely affected by the repair. A wide range of speed and engine-power combi nation must be covered during this check.
b. Fit and Alignment. When making re pairs to wing and tail surface brace members, ensure to proper fit and alignment to avoid distortion.
4-102. LANDING GEAR REPAIR.
a. Round Tube Construction. R e p a i r landing gears made of round tubing using standard repairs and splices as shown in fig ure 4-35 and figure 4-41.
b. Streamline Tube Construction. R e p a i r landing gears made of streamlined tubing by either one of the methods shown in fig ure 4-42, figure 4-44, or figure 4-45.
c. Axle Assemblies. Representative types of repairable and nonrepairable landing gear axle assemblies are shown in figures 4-46 and 4-47.
The types as shown in A, B, and C of this fig ure are formed from steel tubing and may be repaired by the applicable method Par 4-99 Page 4-73
A- Slot Width (Original Tube).
B- Outside Diameter (Insert Tube).
C- Streamline Tube Length of Major Axis.
S.L. Size A B C D 1” .375 .563 1.340 .496 1-¼ .375 .688 1.670 .619 1-½ .500 .875 2.005 .743 1-¾ .500 1.000` 2.339 .867 2 .500 1.125 2.670 .991 2-¼ .500 1.250 3.008 1.115 2-½ .500 1.375 3.342 1.239
ROUND INSERT TUBE (B) SHOULD BE AT LEAST OF SAME MATERIAL AND ONE GAUGE THICKER THAN ORIGINAL STREAMLINE TUBE (C).
FIGURE 4-42. Streamline tube splice using round tube (applicable to landing gear).
d. shown in figure 4-35 through figure 4-45.
However, it will always be necessary to ascer tain whether or not the members are heat treated. The axle assembly as shown in fig ure 4-47 is, in general, of a nonrepairable type for the following reasons.
(1) The axle stub is usually made from a highly heat-treated nickel alloy steel and care fully machined to close tolerances. These stubs are usually replaceable and must be re placed if damaged.
(2) The oleo portion of the structure is gen erally heat treated after welding, and is per fectly machined to ensure proper functioning of the shock absorber. These parts would be distorted by welding after machining.
4-103. REPAIRS TO WELDED ASSEM BLIES. These repairs may be made by the following methods.
a. A welded joint may be repaired by cut ting out the welded joint and replacing it with one properly gusseted. Standard splicing pro cedures should be followed.
Page 4-74 Par 4-102