5-45. PREPARATION OF SURFACE.
a. Remove protective coatings according to the manufacturer’s instructions if necessary.
Unless otherwise specified, magnetic particle examination should not be performed with coatings in place that could prevent the detection of surface defects in the ferro-magnetic substrate. Such coatings include paint or chromeplate thicker than 0.003 inch, or ferromagnetic coatings such as electroplated nickel thicker than 0.001 inch.
b. Parts should be free of grease, oil, rust, scale, or other substances which will interfere with the examination process. If re - quired, clean by vapor degrease, solvent, or abrasive means per the manufacturer’s in - structions. Use abrasive cleaning only as necessary to completely remove scale or rust. Ex - cessive blasting of parts can affect examination results.
c. Exercise extreme care to prevent any cleaning material or magnetic particles from becoming entrapped where they cannot be removed. This may require extracting components such as bushings, bearings, or inserts from assemblies before cleaning and magnetic particle examination.
d. A water-break-free surface is re - quired for parts to be examined by water suspension methods. If the suspension completely wets the surface, this requirement is met.
e. Magnetic particle examination of assembled bearings is not recommended because the bearings are difficult to demagnetize. If a bearing cannot be removed, it should be protected from the magnetic particle examination materials and locally magnetized with a mag - netic yoke to limit the magnetic field across the bearing.
5-46. METHODS OF EXAMINATION.
Magnetic particle examination generally consists of: the application of magnetic particles;
magnetization; determination of field strength;
special examination techniques; and demag - netization and post-examination cleaning.
Each of these steps will be described in the following paragraphs.
5-47. APPLICATION OF MAGNETIC PARTICLES. The magnetic particles used can be nonfluorescent or fluorescent (dependent on the examination required) and are applied suspended in a suitable substance. Fluorescent particles are preferred due to their higher sensitivity.
a. Wet Continuous Method. Unless otherwise specified, use only the wet continuous method. In the wet continuous method, the particle suspension is liberally applied to wet all surfaces of the part. The magnetizing current is applied at the instant the suspension is diverted from the part. Apply two shots of magnetizing current, each at least 1/2 second long.
(1) Wet suspensions of fluorescent particles, either in water or oil, should be used for most overhaul and in-service examinations ex - cept where the material, size, or shape of the part prohibits its use.
(2) Water, with a suitable rust inhibitor and wetting agent, may be used as a liquid ve - hicle, provided that magnetic examination equipment is designed for use or is satisfactorily converted for use with water.
b. Dry Continuous Method. T h i s method is not recommended for use on aerospace components because of its lower sensitivity level.
Page 5-22 Par 5-45
c. Residual Magnetization Method. In this method, the part is magnetized and the magnetizing current is then cut off. If the amperage has been correctly calculated and qual - ity indicator has verified the technique, then one shot will correctly magnetize the part. The magnetic particles are applied to the part after the magnetization. This method is dependent upon the retentiveness of the part, the strength of the applied field, the direction of magnetization, and the shape of the part.
5-48. MAGNETIZATION.
a. Circular. Circular magnetization is induced in the part by the central-conductor method or the direct-contact method. (See fig - ure 5-11.)
(1) Indirect Induction (central-conductor method). Pass the current through a central conductor that passes through the part. When several small parts are examined at one time, provide sufficient space between each piece to permit satisfactory coverage (with particles), magnetization, and examination.
(2) Direct Induction (contact method).
Pass current through the part mounted horizontally between contact plates. As an exam - ple, circular magnetization of a round steel bar would be produced by placing the ends of the steel bar between the heads of the magnetic in - spection machine and passing a current through the bars. Magnetic particles applied either during or after passage of the current, or after passage of the current in magneticallyretentive steels, would disclose discontinuities parallel to the axis of the bar.
NOTE: Exercise extreme caution to prevent burning of the part at the electrode contact areas. Some causes of overheating and arcing are: insuffi - cient contact area, insufficient contact pressure, dirty or coated contact areas, electrode removal during current flow, and too high an amperage setting.
FIGURE 5-11. Circular magnetization.
Par 5-47 Page 5-23
b. Longitudinal. Longitudinal magnetization is induced in a part by placing the part in a strong magnetic field, such as the center of a coil or between the poles of an electromagnetic yoke. (See figure 5-12.) When using a coil, optimum results are obtained when the
(3) The area of the coil opening is at least 10 times the cross-sectional areas of the part.
(4) The part is positioned against the inner wall of the coil.
following conditions are met.
(5) Three to five turns are employed for
(1) The part to be examined is at least hand-held coils formed with cables.
twice as long as it is wide.
(6) For the 10-to-1 fill factor, the effec-
(2) The long axis of the part is parallel tive region of inspection is 1 coil radius on eito the axis of the coil opening. ther side of the coil with 10 percent overlap.
(Refer to ASTME-1444.)
Cable- Magnetizing current Coll Crack May be permanent or Path of flexible cable- surren magnetizing surren current Magnetic fielo- Coil shot Magnetic lines of force Cable wrap
• Transverse crack will show
- 45° crack will show Current Yoke Longitudinal crack will not show Longitudinal magnetic Weld field Yoke Test article
COIL SHOT CABLE WRAP The usual way to longitudinally magnetize a Cable wrapping a coil around large or heavy parts is part is to place the part lengthwise inside the a common practice. Cable length must be kept as necessary on long parts because the effective field extends only 6 to 9 inches on either side of bottom of the coil. Multiple inspections are the coil. short as practical to minimize cable-resistance loss and aid in obtaining higher current amperages. Normally, three to five turns are sufficient.
YOKE Essentially a yoke is a temporary horseshoe magnet.
It is made of low-retentivity iron that is magnetized by a small coil wound around its horizontal bar. Yokes are recommended for parts subject to arc burns and for spot inspection of large parts.
FIGURE 5-12. Longitudinal magnetization.
Page 5-24 Par 5-48
(7) The intensity of the longitudinal shots is kept just below the level at which leakage fields develop across sharp changes of section, such as radii under bolt heads, threads, and other sharp angles in parts. This does not apply when checking chrome-plated parts for grinding cracks.
(a) For example, longitudinal mag - netization of a round steel bar would be produced by placing the DC coil around the bar.
After application of the magnetic particles, ei - ther during or subsequent to magnetization, discontinuities perpendicular to the longitudinal axis of the bar would be disclosed.
(b) When a yoke is used, the portion of the part between the ends of the yoke completes the path of the magnetic lines of force.
This results in a magnetic field between the points of contact.
c. Permanent Magnets and Electromagnetic Yoke. The stability of the magnetic field generated by permanent magnets requires some agitation of the oxide particles within the field. The wet method is considered most satisfactory. Use a well-agitated plastic squirt bottle for the most effective application of the magnetic particle suspension. When the direction of possible cracks in a suspect area is not known, or would not necessarily be normal to the lines of force between the poles of the magnet, reposition the magnet to the best ad - vantage and recheck. Usually, two shots, 90 degrees apart are required. The part must be demagnetized between each magnetization when the field direction is changed unless the next shot is at least 10 percent stronger than the previous shot, if this is the case demagnetization is not necessary.
5-49. DETERMINATION OF FIELD STRENGTH. Factors such as part size, shape, magnetic properties of the material, and the method of magnetization will affect the field strength induced within a part by a given applied magnetizing force. The factors vary considerably, making it difficult to establish rules for magnetizing during examination.
Technique requirements are best determined on actual parts having known defects.
a. A magnetization indicator, such as a Quantitative Quality Indicator (QQI), should be used to verify that adequate magnetic flux strength is being used. It effectively indicates the internally-induced field, the field direction, and the quality of particle suspension during magnetization.
b. The level of magnetization required for detection of service-related defects in most cases can be lower than that required for mate - rial and manufacturing control. Contact the manufacturer for correct specifications.
NOTE: If the examination must be performed with less current than is desired because of part size or equip - ment limitations, the lower field strength can be partially accommo - dated by reducing the area of exami - nation for each magnetization, or the examination can be supplemented by using electromagnetic yokes. Examine only 4 inches on either side of a coil instead of 6, or apply additional magnetization around the periphery of a hollow cylinder when using an inter - nal conductor.
5-50. SPECIAL EXAMINATION TECH- NIQUES.
a. Magnetic Rubber. Magnetic rubber formulations using finely divided magnetic particles in a silicone rubber base are used for the inspection of screw, bolt, or other bore holes, which are not easily accessible. The liquid silicone rubber mixture is poured into holes in magnetic parts to be inspected.
Par 5-48 Page 5-25
Curing time for silicone rubbers varies from about 30 minutes and up depending upon the particular silicone rubber, the catalyst, and the amount of catalyst used to produce the curing reaction.
b. Curing. While curing is taking place, the insides of the hole must be maintained in the required magnetized state. This can be accomplished using a permanent magnet, a DC yoke, an electromagnet, or some other suitable means. Whatever method of magnetization is used, the leakage fields at any discontinuities inside the holes must be maintained long enough to attract and hold in position the mag - netic particles until a partial cure takes place.
A two-step magnetizing procedure has been developed.
(1) The first magnetization is accom - plished for a short time in one direction followed by a second at 90 degrees to the first for the same length of time. This procedure must be repeated for whatever period of time is needed until the cure prevents particle mobility. Magnetization in two directions 90 degrees apart ensures formation of indications at discontinuities in all directions inside the holes.
(2) After curing, the rubber plugs, which are exact replicas of the holes, are removed and visibly examined for indications which will appear as colored lines against the lighter colored background of the silicone rubber. Location of any discontinuities or other surface imperfections in the holes can be determined from the location of the indications on the plugs. The magnetic rubber inspection method is covered in detail in Air Force Technical Order 33B-1-1, section XI.
c. Critical Examination for Sharp Radii Parts. A critical examination is required for cracks in sharp radii; such as threaded parts, splines, gear teeth roots, and abrupt changes in sections, that cause obscuring and nonrelevant indications during normal examination practices. The procedure provided herein is the most sensitive method for detecting the early beginnings of in-service fatigue cracks in the sharp, internal radii of ferro-magnetic parts.
Magnetic particle examination equipment may be used; however, alternating fields are not reliable to provide the necessary high level of residual magnetism. Optical aids are necessary to realize the maximum sensitivity provided by this magnetic particle procedure. Low-power (10x-30x) binocular microscopes are recommended. As a minimum, pocket magnifiers of 7 to 10 power may be used with the following procedure.
(1) Thoroughly clean the part at the sharp radii and fillets where soils, greases, and other contaminants tend to accumulate and at other places where they might be overlooked during a casual or hasty examination.
(2) The residual method should be used as an aid in particular problem areas, even though it is not considered the best practice in most of the instances. The conventional wet continuous methods should be used initially for overall examination and the residual tech - nique should be applied only for supplemental, local examination of the sharp radii. It should not be applied except in those cases where nonrelevant indications have proven to be a problem in the initial examination.
(3) Methods of magnetization should be done according to standard procedures; however, alternating fields should not be used, and the level of magnetizing force imposed should usually be increased above the normal levels to ensure a higher residual field within the part.
(4) Following magnetization, apply particles in liquid suspension. The application should be liberal and in a manner to cause maximum particle buildup. Immersion of Page 5-26 Par 5-50
small parts such as rod end fittings in a container of suspension, which has just been stirred for about 30 seconds, is an excellent method.
(5) Check for the presence of particle accumulation in the sharp radii. It is necessary that the level of magnetization and the particle application result in the formation of nonrelevant indications. Lack of indications will re - quire remagnetization to a higher level, more care in applying the particles, or both.
(6) Wash the parts in a clean suspension vehicle only enough to remove the weaklyheld particle accumulations causing the nonrelevant indications. Particles at true cracks will be more strongly held and will persist if the washing is gently done. This can be accomplished by flowing or directing a stream of liquid vehicle over the part, or for a small component, by gently stirring in a container of the vehicle. Closely observe the removal of the nonrelevant particle accumulations in the region to be examined to avoid excessive washing. If washing is prolonged beyond the minimum needed to remove the nonrelevant indications, the small defect indications may also be washed away. A few trials will help to develop the best method and time required for washing.
(7) Check for crack indications with optical magnification and ample lighting. The smaller indications that are attainable by this procedure cannot be reliably seen or evaluated with the unaided eye.
5-51. DEMAGNETIZATION AND POST - EXAMINATION CLEANING . Parts should be magnetized longitudinally last before demagnetizing.
NOTE: Circular magnetism cannot be read with a field meter since it is an internal magnetic field. However, if the last shot, was a coil shot the meter can read it if a magnetic field is pres - ent.
a. Demagnetization. Demagnetize be - tween successive magnetization of the same part, to allow finding defects in all directions, and whenever the residual magnetism inter - feres with the interpretation of the indications.
Also, demagnetize all parts and materials after completion of magnetic particle examination.
Test all parts at several locations and parts for residual magnetism of complex configuration at all significant changes in geometry. Repeat demagnetization if there is any appreciable de - flection of the field indicator needle.
(1) AC method. Hold the part in the AC demagnetizing coils and then move the part slowly and steadily through the coils and approximately 3 to 4 feet past the coils. Re - peat this process until the part loses its residual magnetism. Rotate and tumble parts of complex configuration as they are passed through the coils.
(2) DC method. Place the part in the same relative position as when magnetized and apply reversing DC current. Gradually reduce the current to zero and repeat the process until the residual magnetic field is depleted.
b. Post-Examination Cleaning.
(1) When oil suspensions are used, sol - vent clean or remove the part until all magnetic particles and traces of oil are removed.
Par 5-50 Page 5-27
(2) When parts or materials have been examined using water suspension methods, completely remove the water by any suitable means, such as an air blast, to ensure that the parts are dried immediately after cleaning.
Thoroughly rinse the part with a detergentbase cleaner until all magnetic particles are removed. Then rinse in a solution of water and rust inhibitor.
(3) For cadmium-plated parts an airwater vapor blast may be used to remove any remaining magnetic particle residue.
(4) After final cleaning and drying, use temporary protective coatings, when necessary, to prevent corrosion.
(5) After magnetic particle examination has been completed, restore any removed finishes according to the manufacturer’s repair manual.
NOTE: Visible penetrant is often used interchangeably by NDI person - nel with fluorescent penetrant. However, the chemical within most com - mon red dye penetrants will neutralize the fluorescence of the chemicals used in that method. Therefore, a thorough cleaning of all magnetic particles is mandatory.
5-52. 5-59. [RESERVED.] Page 5-28 Par 5-51
SECTION 5. PENETRANT INSPECTION
5-60. GENERAL. Penetrant inspection is used on nonporous metal and nonmetal components to find material discontinuities that are open to the surface and may not be evident to normal visual inspection. The part must be clean before performing a penetrant inspection.
The basic purpose of penetrant inspection is to increase the visible contrast between a discontinuity and its background. This is accomplished by applying a liquid of high penetrating power that enters the surface opening of a discontinuity. Excess penetrant is removed and a developer material is then applied that draws the liquid from the suspected defect to reveal the discontinuity. The visual evidence of the suspected defect can then be seen either by a color contrast in normal visible white light or by fluorescence under black ultraviolet light. (See figure 5-13.)
a. The penetrant method does not depend upon ferro-magnetism like magnetic particle inspection, and the arrangement of the discontinuities is not a factor. The penetrant method is effective for detecting surface defects in nonmagnetic metals and in a variety of nonmetallic materials. Penetrant inspection is also used to inspect items made from ferro - magnetic steels and its sensitivity is generally greater than that of magnetic particle inspec - tion. Penetrant inspection is superior to visual inspection but not as sensitive as other ad - vanced forms of tests for detection of in-service surface cracks.
b. The major limitations of the penetrant inspection is that it can detect only those discontinuities that are open to the surface; some other method must be used for detecting subsurface defects. Surface roughness or porosity can limit the use of liquid penetrants. Such surfaces can produce excessive background indications and interfere with the inspection.
Penetrant inspection can be used on most air - frame parts and assemblies accessible to its application. The basic steps to perform penetrant inspections are briefly described in the following paragraphs.
5-61. EQUIPMENT USED IN THE PENETRANT INSPECTION PROCESS.
Equipment varies from simple aerosol cans used in portable systems to fully automated computer-controlled systems. Whether fluorescent or visible penetrants are used, different penetrant bases are available but may require different cleaning methods. Water-washable penetrants can often be removed by a simple water washing process, whereas oil-base penetrants may require special solvents for re - moval. Some oil-base penetrants have emulsifiers, either added to the penetrant before it is applied or added afterwards, that allow water washing to be used. Developers used, can be applied either by a wet or dry bath. Therefore, each penetrant inspection process may require different cleaning facilities and procedures.
(See table 5-3.)
5-62. BASIC STEPS TO PERFORM PENETRATION INSPECTION. Table 5-4 shows a general process, in the procedures flow sheet, for commonly used penetrant inspection processes. It is important to ensure that parts are thoroughly cleaned and dried before doing penetrant inspection. All surfaces to be inspected should be free of contaminants, paint, and other coatings that could prevent penetrant from entering discontinuities. Ta - ble 5-5 shows applications of various methods of precleaning for penetrant inspection.
Par 5-60 Page 5-29
FIGURE 5-13. Penetrant and developer action.
TABLE 5-3. Classification of penetrant inspection materials covered by MIL-I-25135E.
PENETRANT SYSTEMS DEVELOPERS SOLVENT REMOVERS Type I Type II Type III Fluorescent Dye Visible Dye Visible and Fluorescent Dye (dual mode) Form a Form b Form c Form d Form e Dry Powder Water Soluble Water Suspendible Nonaqueous Specific Application Class (1) Class (2) Class (3) Halogenated (chlorinated) Nonhalogenated (nonchlorinated) Specific Application Method A Method B Method C Method D Water Washable Post emulsifiable, Lipophilic Solvent Removable Post Emulsifiable, Hydrophilic Sensitivity Level 1/2 Sensitivity Level 1 Sensitivity Level 2 Sensitivity Level 3 Sensitivity Level 4 Ultralow Low Medium High Ultrahigh Page 5-30 Par 5-62
TABLE 5-4. Fluorescent and visible penetrant inspection general processing procedures flowsheet.
Penetrant Inspection-General Processing Incoming parts Alkaline Steam Vapor degrease Solvent wash Acid Etch
PRECLEAN Mechanical Paint stripper Ultrasonic Detergent Apply water Apply solvent Apply post PENETRATE washable removable emulsifiable penetrant penetrant penetrant Apply Apply emulsifier remover REMOVE Water wash Solvent wipe-off Pre-rinse Dry (aqueous) Developer (aqueous) Developer DEVELOP Developer Developer (dry or non Developer (dry or non aqueous (dry or non aqueous aqueous) nspect
INSPECT Water finse Detergent Mechanical wash
POST CLEAN Vapor degrease Solvent soak Ultrasonic clean Outgoing parts Par 5-62 Page 5-31
TABLE 5-5. Pre-cleaning methods for penetrant inspection.
METHOD USE Mechanical Methods Abrasive tumbling Dry abrasive grit blasting Wet abrasive grit blast Wire brushing High pressure water and steam Ultrasonic cleaning Chemical Methods Alkaline cleaning Acid cleaning Molten salt bath cleaning Solvent Methods Solvent wiping Removing light scale, burrs, welding flux, braze stopoff, rust, casting mold, and core material; should not be used on soft metals such as aluminum, magnesium, or titanium.
Removing light or heavy scale, flux, stopoff, rust, casting mold and core material, sprayed coatings, carbon deposits: In general, any brittle deposit. Can be fixed or portable (may peen metal over defect).
Same as dry except, where deposits are light, better surface and better control of dimensions are required.
Removing light deposits of scale, flux, and stopoff (may mask defect by displac - ing metal).
Ordinarily used with an alkaline cleaner or detergent; removing typical machine shop contamination, such as cutting oils, polishing compounds, grease, chips, and deposits from electrical discharge machining; used when surface finish must be maintained.
Ordinarily used with detergent and water or with a solvent; removing adhering shop contamination from large quantities of small parts.
Removing braze stopoff, rust, scale, oils, greases, polishing material, and carbon deposits; ordinarily used on large articles where hand methods are too laborious;
also used on aluminum for gross metal removal.
Strong solutions for removing heavy scale; mild solutions for light scale; weak (etching) solutions for removing lightly smeared metal.
Conditioning and removing heavy scale; not suitable for aluminum, magnesium, or titanium.
Same as for vapor degreasing except a hand operation; may employ nonhalogenated (nonchlorinated) solvents; used for localized low-volume cleaning.
Page 5-32 Par 5-62
CAUTION: Improper cleaning meth - ods can cause severe damage or degradation of the item being cleaned.
Personnel must select and apply cleaning processes in accordance with aircraft, engine, propeller, or appliance manufacturer’s recommenda - tions.
5-63. CLEANERS AND APPLICATIONS.
Use a cleaner to remove contaminants from parts prior to the application of penetrant inspection materials. After the inspection is completed, penetrant inspection material residues are removed. The following cleaners are commonly used during the penetrant inspection process.
a. Detergents. Detergent cleaners are water-based chemicals called surfactants, which surround and attach themselves to particles of contaminants allowing them to be washed away.
b. Solvents. Solvents dissolve contaminants such as oils, greases, waxes, sealants, paints, and general organic matter so they can easily be wiped away or absorbed on a cloth.
They are also used to remove Method C penetrant material prior to developer application.
c. Alkalies. Alkaline cleaners are water solutions of chemicals that remove contaminants by chemical action or displacement rather than dissolving the contaminant.
d. Paint Removers. The general types of removers used for conventional paint coatings are solvent, bond release, and disintegrating.
e. Salt Baths. Molten salt baths are used in removing heavy, tightly-held scale and ox - ide from low alloy steels, nickel, and cobaltbase alloys, and some types of stainless steel.
They cannot be used on aluminum, magnesium, or titanium alloys.
f. Acids. Solutions of acids or their salts are used to remove rust, scale, corrosion products, and dry shop contamination. The type of acid used and its concentration depends on the part material and contaminants to be removed.
g. Etching Chemicals. Etching chemicals contain a mixture of acids or alkalies plus inhibitors. They are used to remove a thin layer of surface material, usually caused by a me - chanical process, that may seal or reduce the opening of any discontinuities. The type of etching solution used depends on the part material and condition.
h. Penetrant Application. Apply the penetrant by spraying, brushing, or by completely submerging the part in a container of penetrant. Wait the recommended amount of time after the penetrant has been applied to allow it to enter any discontinuities
(1) Removal of Excess Penetrant. Ex - cess penetrant must be removed from the part’s surface to prevent a loss of contrast between indications of discontinuities and the background during the inspection. Removal may require actually washing or spraying the part with a cleansing liquid, or may simply require wiping the part clean with a solventmoistened cloth. The removal method is determined by the type of penetrant used.
(2) Drying. If removal of the excess penetrant involves water or other cleaning liquids, drying of the part may be required prior to developer application. When drying is required, the time can be decreased by using ovens or ventilation systems.
i. Developer Application. Apply developer after excess penetrant is removed and, where required, the surface is dried. Apply the developer in a thin uniform layer over the surface to be inspected. Developer acts like a Par 5-62 Page 5-33