AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 260–271
Page 272Open in PDF

CHAPTER 6. CORROSION, INSPECTION & PROTECTION

SECTION 1. GENERAL

6-1. GENERAL. The purpose of this chap­ ter is to provide information that will help maintenance personnel prevent, control, iden­ tify, and treat various types of corrosion. (Re­ fer to AC 43-4A, Corrosion Control For Air­ craft for a more in-depth study on the detection and treatment of corrosion.)

a. Corrosion is a natural occurrence that attacks metal by chemical or electrochemical action and converts it back to a metallic com­ pound.

b. Four conditions must exist before electrochemical corrosion can occur. (See fig­ ure 6-1.) They are:

(1) A metal subject to corrosion (An­ ode);

(2) A dissimilar conductive material (Cathode), which has less tendency to corrode;

(3) Presence of a continuous, conduc­ tive liquid path (Electrolyte); and

(4) Electrical contact between the anode and the cathode (usually in the form of metal­ to-metal contact such as rivets, bolts, and cor­ rosion).

c. Elimination of any one of these condi­ tions will stop electrochemical corrosion. (See figure 6-2.)

NOTE: Paint can mask the initial stages of corrosion. Since corrosion products occupy more volume than the original metal, painted surfaces should be inspected often for irregularities such as blisters, flakes, chips, and lumps.

6-2. FACTORS INFLUENCING COR- ROSION.

a. Some factors which influence metal corrosion and the rate of corrosion are:

(1) Type of metal;

(2) Heat treatment and grain direction;

(3) Presence of a dissimilar, less corro­ dible metal;

(4) Anodic and cathodic surface areas (in galvanic corrosion);

(5) Temperature;

(6) Presence of electrolytes (hard water, salt water, battery fluids, etc.);

(7) Availability of oxygen;

(8) Presence of biological organisms;

(9) Mechanical stress on the corroding metal; and,

(10) Time of exposure to a corrosive environment.

(11) Lead/graphite pencil marks on air­ craft surface metals.

b. Most pure metals are not suitable for aircraft construction and are used only in com­ bination with other metals to form alloys.

Most alloys are made up entirely of small crystalline regions, called grains. Corrosion can occur on surfaces of those regions which Par 6-1 Page 6-1

Page 273Open in PDF

are less resistant and also at boundaries be­ tween regions, resulting in the formation of pits and intergranular corrosion. Metals have a wide range of corrosion resistance. The most active metals, (those which lose electrons eas­ ily), such as magnesium and aluminum, cor­ rode easily. The most noble metals (those which do not lose electrons easily), such as gold and silver, do not corrode easily.

FIGURE 6-1. Simplified corrosion cell showing conditions which must exist for electrochemical corrosion.

FIGURE 6-2. Elimination of corrosion by application of an organic film to metal surface.

Page 6-2 Par 6-2

Page 274Open in PDF

c. Corrosion is quickened by hightemperature environments that accelerate chemical reactions and increase the concentra­ tion of water vapor in the air.

d. Electrolytes (electrically-conducting solutions) form on surfaces when condensa­ tion, salt spray, rain, or rinse water accumulate.

Dirt, salt, acidic gases, and engine exhaust gases can dissolve on wet surfaces, increasing the electrical conductivity of the electrolyte, thereby increasing the rate of corrosion.

e. When some of the electrolyte on a metal surface is partially confined, (such as between faying surfaces or in a deep crevice) the metal around this area corrodes more rap­ idly. This type of corrosion is called an oxygen concentration cell. Corrosion occurs more rapidly because the reduced oxygen content of the confined electrolyte causes the adjacent metal to become anodic to other metal surfaces on the same part that are immersed in electro­ lyte or exposed to air.

f. Slime, molds, fungi, and other living organisms (some microscopic) can grow on damp surfaces. Once they are established, the area usually remains damp, increasing the pos­ sibility of corrosion.

g. Manufacturing processes such as ma­ chining, forming, welding, or heat treatment can leave residual stress in aircraft parts and can cause cracking in a corrosive environment.

6-3. COMMON CORROSIVE AGENTS.

Substances that cause corrosion are called cor­ rosive agents. The most common corrosive agents are acids, alkalies, and salts. The at­ mosphere and water, the two most common media for these agents, may also act as corro­ sive agents.

structive are sulfuric acid (battery acid), halo­ gen acids (hydrochloric, hydrofluoric, and hy­ drobromic), nitrous oxide compounds, and or­ ganic acids found in the wastes of humans and animals.

b. Alkalies, as a group, are not as corro­ sive as acids. Aluminum and magnesium al­ loys are exceedingly prone to corrosive attack by many alkaline solutions unless the solutions contain a corrosion inhibitor. Substances par­ ticularly corrosive to aluminum are washing soda, potash (wood ashes), and lime (cement dust).

c. The major atmospheric corrosive agents are oxygen and airborne moisture.

Corrosion often results from the direct action of atmospheric oxygen and moisture on metal nd the presence of additional moisture often accelerates corrosive attack, particularly on ferrous alloys. The atmosphere may also con­ tain other corrosive gases and contaminants, particularly industrial and marine salt spray.

d. The corrosiveness of water depends on the type and quantity of dissolved mineral and organic impurities and dissolved gasses (particularly oxygen) in the water. One char­ acteristic of water that makes it corrosive is its conductivity. Physical factors, such as water temperature and velocity also have a direct bearing on its corrosiveness.

6-4. MICRO-ORGANISMS.

a. Bacteria may be either aerobic or an­ aerobic. Aerobic bacteria require oxygen to live. They accelerate corrosion by oxidizing sulfur to produce sulfuric acid. Bacteria living adjacent to metals may promote corrosion by depleting the oxygen supply or by releasing metabolic products. Anaerobic bacteria, on the other hand, can survive only when free oxygen

a. Any acid will severely corrode most of the alloys used in airframes. The most de- Par 6-2 Page 6-3

Page 275Open in PDF

is not present. The metabolism of these bacte­ ria requires them to obtain part of their suste­ nance by oxidizing inorganic compounds, such as iron, sulfur, hydrogen, and carbon monox­ ide. The resultant chemical reactions cause corrosion.

b. Fungi are the growths of micro­ organisms that feed on organic materials.

While low humidity does not kill microbes, it slows their growth and may prevent corrosion damage. Ideal growth conditions for most mi­ cro-organisms are temperatures between 68 and 104 °F (20 and 40 °C) and relative hu­ midity between 85 and 100 percent.

c. Damage resulting from microbial growth can occur when any of three basic mechanisms, or a combination of these, is brought into play. First, fungi have a tendency to hold moisture, which contributes to other forms of corrosion. Second, because fungi are living organisms, they need food to survive.

This food is obtained from the material on which the fungi are growing. Third, these mi­ cro-organisms secrete corrosive fluids that at­ tack many materials, including some that are not fungi nutrient.

d. Microbial growth must be removed completely to avoid corrosion. Microbial growth should be removed by hand with a firm non-metallic bristle brush and water. Removal of microbial growth is easier if the growth is kept wet with water. Microbial growth may also be removed with steam at 100 psi. Pro­ tective clothing must be used when using steam for removing microbial growth.

6-5.  6-10. [RESERVED.] Page 6-4 Par 6-4

Page 276Open in PDF

SECTION 2. TYPES OF CORROSION

6-11. GENERAL. All corrosive attacks be­ gin on the surface of the metal making the classification of corrosion by physical appear­ ance a convenient means of identification.

(See figure 6-3.)

FIGURE 6-3. Corrosion attack.

6-12. GENERAL SURFACE CORRO- SION. General surface corrosion (also re­ ferred to as Uniform Etch or Uniform Attack Corrosion) is the most common form of corro­ sion and results from a direct chemical attack on a metal surface and involves only the metal surface. (See figure 6-4.) General surface cor­ rosion usually occurs over a wide area and is more or less equal in dispersion. On a pol­ ished surface, this type of corrosion is first seen as a general dulling of the surface, and if allowed to continue, the surface becomes rough and possibly frosted in appearance. The discoloration or general dulling of metal cre­ ated by exposure to elevated temperatures is not to be considered general surface corrosion.

6-13. PITTING CORROSION. Pitting corrosion is one of the most destructive and intense forms of corrosion. It can occur in any metal but is most common on metals that form protective oxide films, such as aluminum and magnesium alloys. It is first noticeable as a white or gray powdery deposit, similar to dust, which blotches the surface. When the deposit is cleaned away, tiny holes or pits can be seen in the surface. (See figures 6-5(a) and 6-5(b).)

These small surface openings may penetrate deeply into structural members and cause damage completely out of proportion to its sur­ face appearance.

FIGURE 6-5(a). Pitting corrosion (external view).

FIGURE 6-5(b). Pitting corrosion (magnified cross sec­ tion).

FIGURE 6-4. General surface corrosion.

Par 6-11 Page 6-5

Page 277Open in PDF

6-14. CONCENTRATION CELL COR- ROSION. Concentration cell corrosion, (also known as Crevice Corrosion) is corrosion of metals in a metal-to-metal joint, corrosion at the edge of a joint even though the joined met­ als are identical, or corrosion of a spot on the metal surface covered by a foreign material.

Metal ion concentration cells and oxygen con­ centration cells are the two general types of concentration cell corrosion. (See figure 6-6.)

a. Metal Ion Concentration Cells . The solution may consist of water and ions of the metal which is in contact with water. A high concentration of the metal ions will normally exist under faying surfaces where the solution is stagnant, and a low concentration of metal ions will exist adjacent to the crevice which is created by the faying surface. An electrical potential will exist between the two points; the area of the metal in contact with the low con­ centration of metal ions will be anodic and corrode, and the area in contact with the high metal ion concentration will be cathodic and not show signs of corrosion.

b. Oxygen Concentration Cells. T h e solution in contact with the metal surface will normally contain dissolved oxygen. An oxy­ gen cell can develop at any point where the oxygen in the air is not allowed to diffuse into the solution, thereby creating a difference in oxygen concentration between two points.

Typical locations of oxygen concentration cells are under gaskets, wood, rubber, and other materials in contact with the metal sur­ face. Corrosion will occur at the area of low oxygen concentration (anode). Alloys such as stainless steel are particularly susceptible to this type of crevice corrosion.

6-15. ACTIVE-PASSIVE CELLS. Metals which depend on a tightly adhering passive film, usually an oxide, for corrosion protection are prone to rapid corrosive attack by activepassive cells. Active-passive cells are often re­ ferred to as a type of concentration cell corro­ sion. However, the active-passive cell is actu­ ally two forms of corrosion working in con­ junction. The corrosive action usually starts as an oxygen concentration cell. As an example, salt deposits on the metal surface in the pres­ ence of water containing oxygen can create the oxygen cell. The passive film will be broken beneath the salt crystals. Once the passive film is broken, the active metal beneath the film will be exposed to corrosive attack. (See figure 6-7.) Rapid pitting of the active metal will result. This reaction can become locally intense due to several factors. First the reac­ tion is augmented by the affected area, since the proportion of the exposed base metal is small compared to the surrounding non­ reactive metal. This effectively concentrates the focal point of the reaction, often resulting in deep pits in a short time and a greater rate of corrosion.

FIGURE 6-6. Concentration cell corrosion.

Page 6-6 Par 6-14

Page 278Open in PDF

6-16. FILIFORM CORROSION. Filiform corrosion is a special form of oxygen concen­ tration cell which occurs on metal surfaces having an organic coating system. It is recog­ nized by its characteristic worm-like trace of corrosion products beneath the paint film.

(See figure 6-8.) Polyurethane finishes are es­ pecially susceptible to filiform corrosion. Fili­ form occurs when the relative humidity of the air is between 78 and 90 percent and the sur­ face is slightly acidic. This corrosion usually attacks steel and aluminum surfaces. The traces never cross on steel, but they will cross under one another on aluminum which makes the damage deeper and more severe for alumi­ num. If the corrosion is not removed, the area treated, and a protective finish applied, the cor­ rosion can lead to inter-granular corrosion, es­ pecially around fasteners and at seams. Fili­ form corrosion can be removed using glass bead blasting material with portable abrasive blasting equipment or sanding. Filiform corro­ sion can be prevented by storing aircraft in an environment with a relative humidity below 70 percent, using coating systems having a low rate of diffusion for oxygen and water vapors, and by washing the aircraft to remove acidic contaminants from the surface.

6-17. INTERGRANULAR CORROSION.

Inter-granular corrosion is an attack on the grain boundaries of a metal. A highly magni­ fied cross section of any commercial alloy shows the granular structure of the metal. It consists of quantities of individual grains, and each of these tiny grains has a clearly FIGURE 6-8. Filiform corrosion.

defined boundary which chemically differs from the metal within the grain. The grain boundary and the grain center can react with each other as anode and cathode when in con­ tact with an electrolyte. (See figure 6-9.)

Rapid selective corrosion of the grain bounda­ ries can occur. High-strength aluminum alloys such as 2014 and 7075 are more susceptible to inter-granular corrosion if they have been im­ properly heat-treated and then exposed to a corrosive environment.

6-18. EXFOLIATION CORROSION. Exfoliation corrosion is an advanced form of in­ ter-granular corrosion and shows itself by lift­ ing up the surface grains of a metal by the force of expanding corrosion products occur­ ring at the grain boundaries just below the sur­ face. (See figure 6-10.) It is visible evidence of inter-granular corrosion and is most often seen on extruded sections where grain thick­ ness are usually less than in rolled forms.

FIGURE 6-7. Active-passive cell.

Par 6-16 Page 6-7

Page 279Open in PDF

FIGURE 6-9. Inter-granular Corrosion of 7075-T6 aluminum adjacent to steel fastener.

FIGURE 6-10. Exfoliation corrosion.

6-19. GALV ANIC CORROSION. Gal­ vanic corrosion occurs when two dissimilar metals make contact in the presence of an electrolyte. (See figure 6-11.) It is usually recognizable by the presence of a build-up of corrosion at the joint between the metals.

6-20. STRESS CORROSION CRACKING .

This form of corrosion involves a constant or cyclic stress, acting in conjunction with a damaging chemical environment. The stress may be caused by internal or external loading.

a. Internal stress may be trapped in a part of structure during manufacturing proc­ esses such as cold working or by unequal cooling from high temperatures. Most manu­ facturers follow up these processes with a stress relief operation. Even so, sometimes stress remains trapped. The stress may be ex­ ternally introduced in part structure by rivet­ ing, welding, bolting, clamping, press fit, etc.

If a slight mismatch occurs, or a fastener is over-torque, internal stress will be present.

b. Internal stress is more important than design stress, because stress corrosion is diffi­ cult to recognize before it has overcome the design safety factor. The level of stress varies from point to point within the metal. Stresses near the yield strength are generally necessary to promote stress corrosion cracking. (See fig­ ure 6-12.) However, failures may occur at lower stresses. Specific environments have been identified which cause stress corrosion cracking of certain alloys.

Page 6-8 Par 6-18

Page 280Open in PDF

FIGURE 6-11. Galvanic corrosion of magnesium adjacent to steel fastener.

FIGURE 6-12. Stress corrosion cracking.

(1) Salt solutions and sea water cause stress corrosion cracking of high-strength, heat-treated steel and aluminum alloys.

(2) Methyl alcohol-hydrochloric acid solutions will cause stress corrosion cracking of some titanium alloys.

(3) Magnesium alloys may stresscorrode in moist air.

(4) Stress Corrosion may be reduced by

• applying protective coatings,

• stress relief heat treatments,

• using corrosion inhibitors, or

• controlling the environment.

6-21. FATIGUE CORROSION . Fatigue corrosion involves cyclic stress and a corrosive environment. Metals may withstand cyclic stress for an infinite number of cycles so long as the stress is below the endurance limit of the metal. Once the limit has been exceeded, the metal will eventually crack and fail from metal fatigue. However, when the part or structure undergoing cyclic stress is also exposed to a corrosive environment, the stress level for fail­ ure may be reduced many times. Thus, failure occurs at stress levels that can be dangerously low depending on the number of cycles as­ signed to the life-limited part.

a. Fatigue corrosion failure occurs in two stages. During the first stage the combined action of corrosion and cyclic stress damages the metal by pitting and crack formations to such a degree that fracture by cyclic stress will occur, even if the corrosive environment is completely removed.

b. The second stage is essentially a fa­ tigue stage in which failure proceeds by propa­ gation of the crack (often from a corrosion pit or pits). It is controlled primarily by stress concentration effects and the physical proper­ ties of the metal. Fracture of a metal part due to fatigue corrosion, generally occurs Par 6-20 Page 6-9

Page 281Open in PDF

at a stress level far below the fatigue limit of an uncorroded part, even though the amount of corrosion is relatively small.

6-22. FRETTING CORROSION. Fretting corrosion,(also known as wear corrosion or friction oxidation) can occur at the interface of two highly-loaded surfaces which are not sup­ posed to move against each other. However, vibration may cause the surfaces to rub to­ gether resulting in an abrasive wear known as fretting. (See figure 6 -13.) The protective film on the metallic surfaces is removed by this rubbing action. With continued rubbing, metal particles sheared from the surface of the metal combine with oxygen to form metal ox­ ide. As these oxides accumulate, they cause damage by abrasive action and increased local stress. The most common example of fretting corrosion is the smoking rivet found on engine cowling and wing skins. This is one corrosion reaction that is not driven by an electrolyte, and in fact, moisture may inhibit the reaction.

Application of a lubricant or installation of a fretting-resistant material between the two sur­ faces can reduce fretting corrosion.

FIGURE 6-13. Fretting corrosion.

6-23.  6-28. [RESERVED.] Page 6-10 Par 6-21

Page 282Open in PDF

SECTION 3. CORROSION PROTECTION MEASURES FOR BASIC MATERIALS

6-29. GENERAL. In the repair of aircraft, apply corrosion proofing of the same type or equivalent to that originally applied unless the repair would result in increased susceptibility to corrosion, in which case use additional cor­ rosion protection measures. The following is a list of the most commonly-used corrosionproofing techniques.

6-30. ANODIZING AND RELATED PROCESSES. In anodizing, aluminum alloys are placed in an electrolytic bath causing a thin film of aluminum oxide to form on the surface of the aluminum. This is resistant to corrosion and affords a good paint base. However, other processes, which do not provide as good a cor­ rosive protection as anodizing, are good paint bases. The processes are:

a. Alkaline cleaning followed by chromic acid dip;

b. Alcoholic phosphoric acid cleaner; and

c. Alkaline dichromate treatment.

6-31. PLATING. Steels are commonly plated with other metals to prevent corrosion.

Plating is accomplished by placing the article in an electrolytic bath. Metals used in plating vary in the corrosion protection they afford steel. For instance, in platings that corrode be­ fore steel, such as zinc or cadmium, slight breaks or cracks throughout the plating will not result in rusting of the exposed steel. With the surface metal corroded, the steel is pro­ tected. However, when the steel corrodes faster than the plate metal, such as chromium, the amount of protection depends on the tight­ ness of the plating. Post-plate bake treatment to relieve hydrogen embrittlement is a neces­ sary part of replating procedures for high-strength steel parts. High-strength nuts and bolts are susceptible to failure from hydro­ gen embrittlement. Because of the potential failures of embrittled parts, careful control over the heat treatment, grinding, preplate cleaning, plating, and post-plate baking of high-strength parts is necessary.

6-32. PHOSPHATE RUST-PROOFING .

This process is commercially known as Parkerizing, Bonderizing, Granodizing, etc.

The coating placed on the part is used to pro­ tect steel parts after machining and before painting.

6-33. CHROME-PICKLE TREATMENT.

Magnesium parts which have been immersed or brushed with a solution of nitric acid and sodium dichromate will be protected for tem­ porary storage. The coating will also serve as a bond for subsequent organic finishes. Sealed chrome-pickle treatment is used on magnesium parts for long term protection. Diluted chro­ mic acid is a touch-up treatment. It is less critical to apply and can be applied over previ­ ously-applied thin chromate films.

6-34. DICHROMATE TREATMENT.

This treatment consists of boiling magnesium parts in a solution of sodium dichromate. It provides good paint base and protective quali­ ties on all standard wrought magnesium alloys except the magnesium-thorium alloys. Acid pickling of the magnesium surface prior to ap­ plication of the dichromate treatment is re­ quired if maximum corrosion resistance of the finish is expected.

6-35. STANNATE IMMERSION TREAT- MENT. Stannate immersion treatment deposits a layer of tin. It is a protective paint base for magnesium alloy parts which contain inserts and fasteners of a dissimilar metal such as Par 6-29 Page 6-11

Page 283Open in PDF

brass, copper, or steel. This treatment cannot be used with parts containing aluminum inserts or fasteners because the high alkalinity of the bath attacks the aluminum.

6-36. GALV ANIC ANODIZING TREAT- MENT. An electrolytic process that provides a paint base and corrosion-preventive film on magnesium alloys containing manganese.

6-37. CLADDING . Aluminum alloys which are susceptible to corrosion are frequently clad with pure aluminum. Slight pits, scratches, or other defects through the cladding material must be avoided, since the aluminum alloy core will corrode rapidly.

6-38. METAL SPRAYING . Metal is melted and sprayed on the surface to be protected.

The surface must be properly prepared and thoroughly cleaned to prevent peeling of the sprayed coat.

6-39. SHOT-PEENING . Shot-peening and other treatments, by which the surface can be placed in compression, are effective in pre­ venting stress corrosion.

6-40. ORGANIC COATINGS. Zinc chro­ mate primer, enamels, chlorinated rubber com­ pounds, etc., are organic coatings commonly used to protect metals.

6-41. DOPE PROOFING. When doped fabrics are applied over an organic finished metal structure, the dope will have a tendency to loosen the finish on the metal. For this rea­ son, organic coatings on the metal are usually covered with a dope-proof paint, with metal foil, or with cellulose tape to prevent the dope from soaking through.

6-42. TUBE INTERIORS. Protect the inte­ riors of structural steel and aluminum tubing against corrosion. A small amount of water entrapped in a tube can corrode entirely through the tube thickness in a short period.

Coat the tube interior by flushing with hot lin­ seed oil, paralketone, or other approved corro­ sion inhibitor. The flushing liquid is usually introduced through small holes drilled in the tubing. Allow the flushing liquid to drain and plug the holes with a screw or by other means to prevent entry of moisture. Air and water­ tight sealing of the tubing will also give ade­ quate protection against corrosion if the tubing is internally dry before being sealed.

6-43.  6-49. [RESERVED.] Page 6-12 Par 6-35