6-135. CORROSION REMOV AL
AROUND COUNTERSUNK FASTENERS IN ALUMINUM ALLOY. Intergranular cor rosion in aluminum alloys often originates at countersunk areas where steel fasteners are used.
a. When corrosion is found around a fixed fastener head, the fastener must be re moved to ensure corrosion removal. All cor rosion must be removed to prevent further cor rosion and loss of structural strength. To re duce the recurrence of corrosion, the panel should receive a chemical conversion coating, be primed, and have the fasteners installed wet with sealant.
b. Each time removable steel fasteners are removed from access panels, they should be inspected for condition of the plating. If mechanical or plating damage is evident, re place the fastener. One of the following fas tener installation methods should be used:
(1) Brush a corrosion-preventive com pound on the substructure around and in the fastener hole, start the fastener, apply a bead of sealant to the fastener countersink, set and torque the fastener within the working time of the sealant (this is the preferred method).
(2) Apply the corrosion preventive compound to the substructure and fastener, set and torque the fastener.
(3) Apply a coating of primer to the fastener, and while wet with primer, set and torque the fastener.
6-136. EXAMPLES OF REMOVING
CORROSION FROM ALUMINUM AND ALUMINUM ALLOYS.
a. Positively identify the metal as alumi num.
b. Clean the area to be reworked. Strip paint if required.
c. Determine extent of corrosion damage.
d. Remove light to moderate corrosion with one of the following.
(1) Non-Powered Corrosion Removal.
(a) The removal of corrosion prod ucts by hand can be accomplished by use of aluminum grit and silicon carbide abrasive, such as non-woven, non-metallic, abrasive mat (Spec. MIL-A-9962), abrasive cloth, and pa per. Aluminum wool, fiber bristle brushes, and pumice powder are also acceptable methods.
(b) Stainless steel brush (Spec.
H-B-178, type III, class 2) may be used as long as the bristles do not exceed 0.010 inch in di ameter. After use of this brush the surface should be polished with 60 grit aluminum ox ide abrasive paper, then with 400 grit alumi num oxide paper. Care should be exercised in any cleaning process to avoid breaking the protective film.
(c) Steel wool, emery cloth, steel wire brushes (except stainless steel brush) copper alloy brushes, rotary wire brushes, or severe abrasive materials should not be used on any aluminum surface.
(2) Chemical Corrosion Removal.
(a) The corrosion removal compound aluminum pretreatment MIL-C-38334, an acid material, may be used to remove corrosion products from aluminum alloy materials or items (e.g., skins, stringer, ribs in wings, tub ing, or ducts). MIL-C-38334 is available in two types:
1 Type I Liquid concentrate mate rials should be diluted in accordance with the Page 6-26 Par 6-135
manufacture’s instructions before use. Type I has a 1 year shelf life; therefore it shall not be used after 1 year from the date of manufacture.
2 Type II Powdered concentrate materials should be dissolved in the volume of water specified on the kit. These materials have an indefinite shelf life in the dry state.
Once mixed, they should be used within 90 days.
(b) Mix MIL-C-38334 in wood, plastic, or plastic-lined containers only. Wear acid-resistant gloves, protective mask and protective clothing when working with this acid compound. If acid contacts the skin or eyes, flush immediately with water.
(c) Apply MIL-C-38334 solution by flowing, mopping, sponging, brushing, or wiping. When applying the solution to large areas, begin the application at the lowest area and work upward, applying the solution with a circular motion to disturb the surface film and ensure proper coverage. If pumping is re quired, pumps, valves, and fittings should be manufactured from 18-8 stainless steel or plastic.
CAUTION: When working with MIL-C-38334, keep the solution away from magnesium surfaces. The solu - tion must be confined to the area be - ing treated. All parts and assemblies including cadmium-plated items and hinges susceptible to damage from acid should be masked and/or protected. Also mask all openings leading to the primary structure that could trap the solution and doors or other openings that would allow the solution (uncontrolled) to get into the aircraft or equipment interior. It is a good practice to keep a wet rag on hand at all times, for removal of spills or splashes.
(d) Allow the solution to remain on the surface for approximately 12 minutes and then rinse away with clean tap water. For pit ted or heavily-corroded areas the compound will be more effective if applied warm (140 °F) followed by vigorous agitation with a non-metallic acid-resisting brush or aluminum oxide abrasive nylon mat. Allow sufficient dwell time, 12 to 15 minutes, before rinsing.
After each application examine the pits and/or corroded area to determine if another applica tion is required with a 4 to 10 power magnify ing glass. (Select the power depending on the distance available to make the inspection.)
Corrosion still on the area will appear as a powdery crust slightly different in color than the uncorroded base metal. Darkening of area due to shadows and reaction from the acid re mover should not be considered.
(e) Once the corrosion has been re moved and the area well-rinsed with clean water, a chromate conversion coating such as MIL-C-81706 or MIL -C-5541 alodine 1200, must be applied immediately thereafter.
e. Remove moderate to heavy corrosion with one of the following.
(1) Powered Corrosion Removal.
(a) Where the problem is severe enough to warrant the use of power tools, a pneumatic drill motor driving either an alumi num-oxide-impregnated nylon abrasive wheel, flap brush or rubber grinding wheel may be used with an abrasive value to approximately 120 grit, as needed. Corrosion-removal acces sories, such as flap brushes or rotary files, should be used on one type of metal only. For example, a flap brush used to remove alumi num should not be used to remove magnesium, steel, etc. Pneumatic sanders may be used with disk and paper acceptable for use on alu minum.
Par 6-136 Page 6-27
(b) When mechanically removing corrosion from aluminum, especially aircraft skin thinner than 0.0625 inch, extreme care must be used. Vigorous, heavy, continuous abrasive grinding can generate enough heat to cause metallurgical change. If heat damage is suspected, hardness tests or conductivity tests must be accomplished to verify condition of the metal. The use of powered rotary files should be limited to heavy corrosion and should not be used on skin thinner than
0.0625 inch.
(2) Blasting.
(a) Abrasive blasting may be used on aluminum alloys using glass beads (Spec.
MIL-G-9954) sizes 10 to 13, or grain abrasive (Spec. MIL -G-5634) types I and III may be used as an alternate method of removing cor rosion from clad and non-clad aluminum al loys. Abrasive blasting should not be used to remove heavy corrosion products. Direct pres sure machines should have the nozzle pressure set at 30 to 40 psi for clad aluminum alloys and 40 to 45 psi for non-clad aluminum alloys.
Engineering approval should be obtained prior to abrasive blasting metal thinner than
0.0625 inch.
(b) When using abrasive blasting on aluminum alloys, do not allow the blast stream to dwell on the same spot longer than 15 seconds. Longer dwell times will cause ex cessive metal removal. Intergranular exfolia tion corrosion is not to be removed by abrasive blasting; however, blasting may be used with powered corrosion removal to determine whether all exfoliation corrosion has been re moved.
f. Inspect the area for remaining corro sion. Repeat procedure if any corrosion re mains.
NOTE: If corrosion remains after the second attempt, use a stronger method, e.g., chemical to mechanical.
g. Using a blend ratio of 20:1 (length to depth) blend and finish the corrosion rework area with progressively finer abrasive paper until 400-grit paper is used.
h. Clean reworked area using dry cleaning solvent. Do not use kerosene or any other pe troleum base fuel as a cleaning solvent.
i. Determine depth of faired depressions to ensure that rework limits have not been ex ceeded.
j. Apply chemical conversion coating, MIL-C-81706, immediately after reworking. If 48 hours or more have elapsed since the con version coating was first applied and the primer or final paint system has not yet been applied, then reapply the conversion coating before continuing.
NOTE: These solutions should not be allowed to come in contact with magnesium or high-strength steels (180,000 psi). Do not permit solutions or materials to contact paint thinner, acetone or other combustible material:
FIRE MAY RESULT.
k. Apply paint finish to area.
6-137. 6-147. [RESERVED.] Page 6-28 Par 6-136
SECTION 9. MAGNESIUM AND MAGNESIUM ALLOYS
6-148. GENERAL. Magnesium and mag nesium alloys are the most chemically active of the metals used in aircraft construction and are the most difficult to protect. However, cor rosion on magnesium surfaces is probably the easiest to detect in its early stages. Since mag nesium corrosion products occupy several times the volume of the original magnesium metal destroyed, initial signs show a lifting of the paint films and white spots on the magne sium surface. These rapidly develop into snow-like mounds or even white whiskers.
The prompt and complete correction of the coating failure is imperative if serious struc tural damage is to be avoided.
6-149. TREATMENT OF WROUGHT MAGNESIUM SHEETS AND FORGINGS.
Corrosive attack on magnesium skins will usu ally occur around the edges of skin panels, un derneath hold-down washers, or in areas physically damaged by shearing, drilling, abra sion, or impact. Entrapment of moisture under and behind skin crevices is frequently a con tributing factor. If the skin section can be eas ily removed, this should be accomplished to ensure complete inhibition and treatment.
a. Complete mechanical removal of cor rosion products should be practiced when practical. Mechanical cleaning should nor mally be limited to the use of stiff bristle brushes and similar nonmetallic cleaning tools.
b. Any entrapment of steel particles from steel wire brushes, steel tools, or con tamination of treated surfaces, or dirty abra sives, can cause more trouble than the initial corrosive attack. The following procedural summary is recommended for treatment of cor roded magnesium areas when accomplished under most field conditions.
c. When aluminum insulating washers are used and they no longer fasten tightly to magnesium panels, corrosion is likely to occur under the washers if corrective measures are not taken.
(1) When machine screw fasteners are used, aluminum insulating washers must be removed from all locations to surface treat the magnesium panel.
(2) Where permanent fasteners other than machine screws are used, the insulating washer and fastener must be removed.
(3) When located so water can be trapped in the counter-bored area where the washer was located, use sealants to fill the counterbore. If necessary, fill several areas adjacent to each other. It may be advantageous to cover the entire row of fasteners with a strip of sealant.
6-150. REPAIR OF MAGNESIUM
SHEET METAL AFTER EXTENSIVE CORROSION REMOV AL. The same gen eral instructions apply when making repairs in magnesium as in aluminum alloy skin, except that two coats of epoxy primer may be re quired on both the doubler and skin being patched instead of one. Where it is difficult to form magnesium alloys in the contour, alumi num alloy may be utilized. When this is done, it is necessary to ensure effective dissimilar metal insulation. Vinyl tape will ensure posi tive separation of dissimilar metals, but edges will still have to be sealed to prevent entrance of moisture between mating surfaces at all points where repairs are made. It is recom mended that only non-corrosive type sealant be used, since it serves a dual purpose of material separation and sealing.
Par 6-148 Page 6-29
6-151. IN-PLACE TREATMENT OF MAGNESIUM CASTINGS . Magnesium castings, in general, are more porous and more prone to penetrating attack than wrought mag nesium skin. However, treatment in the field is, for all practical purposes, the same for all magnesium. Bellcranks, fittings, and numer ous covers, plates, and handles may also be magnesium castings. When attack occurs on a casting, the earliest practical treatment is re quired to prevent dangerous corrosive penetra tion. Engine cases in salt water can develop moth holes and complete penetration over night.
a. If at all practical , faying surfaces in volved shall be separated to treat the existing attack effectively and prevent its further prog ress. The same general treatment sequence as detailed for magnesium skin should be fol lowed. Where engine cases are concerned, baked enamel overcoats are usually involved rather than other top coat finishes. A good air drying enamel can be used to restore protec tion.
b. If extensive removal of corrosion products from a structural casting is involved, a decision from the aircraft manufacturer or a DER may be necessary to evaluate the ade quacy of structural strength remaining. Refer to the aircraft manufacturer if any questions of safety are involved.
6-152. EXAMPLE OF REMOVING CORROSION FROM MAGNESIUM . If possible, corroded magnesium parts shall be removed from aircraft. When impossible to remove the part, the following procedure will be used.
a. Positively identify metal as magnesium.
b. Clean area to be reworked.
c. Strip paint if required.
d. Determine the extent of corrosion damage.
e. Remove light to moderate corrosion by one of the following means.
(1) Non-Powered Corrosion Removal.
(a) Non-powered removal can be ac complished using abrasive mats, cloth, and pa per with aluminum oxide grit (do not use sili con carbide abrasive). Metallic wools and hand brushes compatible with magnesium such as stainless steel and aluminum, may be used.
(b) When a brush is used the bristles should not exceed 0.010 inch in diameter.
After using a brush, the surface should be pol ished with 400 grit aluminum oxide abrasive paper, then with 600 grit aluminum oxide abrasive paper.
(c) Pumice powder may be used to remove stains or to remove corrosion on thin metal surfaces where minimum metal removal is allowed.
(2) Chemical Corrosion Removal.
(a) Chemical corrosion removal on magnesium alloys is usually done with a chromic acid pickle solution. Chemical corro sion removal methods are not considered ade quate for areas that have:
1 Deep pitting, 2 Heavy corrosion and corrosion by products, 3 Previously had corrosion re moved by mechanical means, or 4 Previously been sand blasted.
Page 6-30 Par 6-151
(b) Do not use this method for parts containing copper and steel-based inserts (un less the inserts are masked off) and where it might come into contact with adhesive bonded skins or parts.
(3) The following solution may be used to remove surface oxidation and light corro sion products from magnesium surfaces.
(a) Solution Composition and Op eration:
1 Chromium Trioxide. 24 oz.
2 (O-C-303, Type II). Water to Make 1 gal. Reaction Time 1 to 15 min.
3 Operation Temperature. (Solu tion can be operated at room temperature for a longer reaction time if desired.) 190 to 202 °F.
4 Container Construction. Leadlined steel, stainless steel, or 1100 aluminum.
(b) Mask off nearby operating mechanisms, cracks and plated steel to keep the solution from attacking them.
(c) Apply chromic acid solution care fully to the corroded area with an acid-resistant brush.
(d) Allow the solution to remain on the surface for approximately 15 minutes.
Agitation may be required.
(e) Thoroughly rinse the solution from the surface with plenty of clean water.
(f) Repeat the preceding sequence as necessary until all corrosion products have been removed and the metal is a bright metal lic color.
f. Remove moderate to heavy corrosion by one of the following means.
(1) Powered Corrosion Removal.
(a) Powered corrosion removal can be accomplished using pneumatic drill motor with either an aluminum-oxide-impregnated abrasive wheel, flap brush, or rubber grinding wheel with an abrasive value to approximately 120 grain size.
(b) Also a rotary file with fine flutes can be used for severe or heavy corrosion product buildup on metals thicker than
0.0625 inch. If a flap brush or rotary file is used, it should only be used on one type of metal. Do not use either a hand or rotary car bon steel brush on magnesium.
(c) Pneumatic sanders are acceptable if used with disk or paper of aluminum oxide.
When using sanders, use extra care to avoid over heating aircraft skins thinner than
0.0625 inch.
(d) Do not use rotary wire brushes on magnesium.
WARNING: Cuttings and small shavings from magnesium can ignite easily and are an extreme fire hazard.
Fires of this metal must be extin - guished with absolutely dry talc, calcium carbonate, sand, or graphite by applying the powder to a depth of 1/2 inch over the metal.
(2) Blasting. Abrasive blasting is an approved method of corrosion removal on magnesium alloys of a thickness greater than
0.0625 inch. Remove heavy corrosion prod ucts by hand brushing with a stainless steel or fiber brush followed by vacuum abrasive Par 6-152 Page 6-31
blasting with glass beads, (Spec. MIL-G-9954) sizes 10-13; or grain abrasive (Spec.
MIL-G-5634), types I or III at an air pressure of 10 to 35 psi (if suction equipment is used, use a 50 percent higher pressure). Upon com pletion of blasting, inspect for the presence of corrosion in the blast area. Give particular at tention to areas where pitting has progressed into intergranular attack. This is necessary be cause abrasive blasting has a tendency to close up streaks of intergranular corrosion rather than remove them if the operator uses an im proper impingement angle. If the corrosion has not been removed in a total blasting time of 60 seconds on any one specific area, other mechanical methods of removal should be utilized.
CAUTION: When blasting magnesium alloys, do not allow the blast stream to dwell on the same spot longer than 15 seconds. Longer dwell times will cause excessive metal re - moval.
g. Inspect the reworked area to ensure that no corrosion products remain. If corrosion products are found, repeat method used and re-inspect.
h. Fair depressions resulting from rework using a blend ratio of 20:1. Clean rework area using 240 grit abrasive paper. Smooth with 300 grit and finally polish with 400 grit abra sive paper.
i. Determine depth of faired depressions to ensure that rework limits have not been ex ceeded. Refer to the manufacture’s specifica tions.
j. Clean reworked area using a solvent to provide a water-break-free surface. Do not use kerosene or another petroleum base fuel as a cleaning solvent.
k. Apply Chromic Acid Brush-on Pre treatment.
(1) Chemical pretreatment such as the following chromic acid solution (Conversion coat conforming to Spec. MIL-M-3171, type VI) provides a passive surface layer with an inhibitive characteristic that resists corro sive attack and also provides a bond for subse quent coatings. Properly-applied magnesium pretreatment tend to neutralize corrosion me dia in contact with the surface.
(2) The chromic acid brush-on pre treatment may be applied to all magnesium parts that require touch-up. This treatment is generally used in refinishing procedures or when parts and assemblies are too large to be immersed. This treatment is less critical to ap ply than the other brush-on treatments. It is relatively inexpensive and not as harmful when trapped in faying surfaces.
(a) Solution Composition and Op eration:
1 Distilled Water 1 gal.
2 Chromic Acid (CrO3) 1.3 oz.
3 (99.5 pure), Calcium Sulfate 1 oz. (CaSo4.2H2O) 4 Operating Temp. 70-90 °F.
5 Container: Stainless Steel, Alu minum, Vinyl, Polyethylene, or Rubber.
NOTE: Good application requires proper preparation of the chromic acid coating solution and cleaning of the surface where the solution will be applied. A water-break test is recom - mended if the cleanliness of the surface is in doubt.
Page 6-32 Par 6-152
(b) Add chemicals to water in the or der shown.
(c) Stir vigorously for at least 15 minutes, either mechanically or by air agi tation, to ensure that the solution is saturated with calcium sulfate. (Let solution stand for 15 minutes before decanting.)
(d) Prior to use, decant solution (avoid transfer of undissolved calcium sulfate) into suitable containers (polyethylene or glass).
(e) Apply solution by brush, swab, or flow on using low-pressure spray (non atomizing) until the metal surface becomes a dull color (the color can vary from greenbrown, brassy, yellow-brown to dark-brown).
For good paint adhesion, a dark-brown color free of powder is considered best. The color may vary in using different vendors’ materials.
NOTE: Too long an exposure to the brush-on solution produces coatings that will powder and impair adhesion of applied paint finish/films.
(f) Observe the coating closely dur ing the treatment for color changes, rinsed with cold running water when the desired condi tion/color is reached and air dried. Preparation and use of test panels made of the same mate rial and under the same conditions, before starting the actual treating operation may be used as to determine the application time re quired to produce the required coating. A good coating is uniform in color/density, ad heres well and is free of loose powder.
l. Apply primer and top coat finish
m. Remove masking and protective cov erings.
6-153. 6-163. [RESERVED.] Par 6-152 Page 6-33 (and 6-34)
SECTION 10. FERROUS METALS
6-164. GENERAL. One of the most famil iar kinds of corrosion is red iron rust. Red iron rust results from atmospheric oxidation of steel surfaces. Some metal oxides protect the un derlying base metal, but red rust is not a pro tective coating. Its presence actually promotes additional attack by attracting moisture from the air and acts as a catalyst to promote addi tional corrosion.
a. Red rust first shows on bolt heads, hold down nuts, and other unprotected aircraft hardware. Red rust will often occur under nameplates that are secured to steel parts. Its presence in these areas is generally not dan gerous. It has no immediate effect on the structural strength of any major components.
However, it shows a general lack of mainte nance and may indicate attack in more critical areas.
b. When paint failures occur or me chanical damage exposes highly-stressed steel surfaces to the atmosphere, even the smallest amount of rusting is potentially dangerous and should be removed immediately.
6-165. SPECIAL TREATMENT OF HIGH-STRENGTH STEEL. (High-strength steels heat treated above Rockwell C40, 180,000 psi tensile strength). Any corrosion on the surface of a highly-stressed steel part is potentially dangerous, and the careful removal of corrosion products is mandatory. Surface scratches or change in surface structure from overheating can cause sudden failure of these parts. The removal of corrosion products is required and will be performed carefully and completely.
a. Acceptable methods include careful use of mild abrasive mats, cloths, and papers, such as fine grit aluminum oxide, metallic wool, or fine buffing compounds.
b. Undesirable methods include the use of any power tool because the danger of local overheating and the formation of notches that could lead to failure. The use of chemical cor rosion removers is prohibited, without engi neering authorization, because high-strength steel parts are subject to hydrogen embrittle ment.
6-166. SPECIAL TREATMENT OF STAINLESS STEEL. Stainless steels are of two general types: magnetic and nonmagnetic.
a. Magnetic steels are of the ferritic or martensitic types and are identified by num bers in the 400-series. Corrosion often occurs on 400-series stainless steels and treatment is the same as specified in high-strength steels.
(See paragraph 6-165.)
b. Non-magnetic stainless steels are of the austenitic type and are identified by num bers in the 300-series. They are much more corrosion resistant than the 400-series steels, particularly in a marine environment.
(1) Austenitic steels develop corrosion resistance by an oxide film, which should not be removed even though the surface is discol ored. The original oxide film is normally formed at time of fabrication by passivation. If this film is broken accidentally or by abrasion, it may not restore itself without repassivation.
(2) If any deterioration or corrosion does occur on austenitic steels, and the struc tural integrity or serviceability of the part is af fected, it will be necessary to remove the part.
Par 6-164 Page 6-35
6-167. EXAMPLE OF REMOVING
CORROSION FROM FERROUS MET - ALS. If possible, corroded steel parts should be removed from the aircraft. When impracti cal to remove the part, follow the procedure below.
a. Prepare the area for rework.
b. Positively identify the metal as steel and establish its heat-treated value.
c. Clean the area and strip paint if re quired.
NOTE: Use of acid-based strippers, chemical removers, or chemical con - version coatings are not permitted on steel parts without engineering authorization.
d. Determine extent of corrosion damage.
e. Remove residual corrosion by hand sanding with mild abrasive mats, cloths, and papers, such as fine aluminum oxide grit.
f. Remove heavy deposits of corrosion products by approved mechanical methods for that particular form of steel and/or stainless steel.
g. Inspect the area for remaining corro sion. Repeat procedure if any corrosion re mains and the structural integrity of the part is not in danger, and the part meets the rework limits established by the manufacturer or FAA authorized DER.
h. Fair depressions using a blend ratio of 20:1. Clean area using 240-grit paper.
Smooth area with 300-grit paper and give final polish with 400-grit paper.
i. Determine depth of faired depression to ensure that rework limits have not been ex ceeded.
j. Clean reworked area with dry cleaning solvent. Do not use kerosene.
k. Apply protective finish or specific or ganic finish as required.
NOTE: Steel surfaces are highlyreactive immediately following corrosion removal; consequently, primer coats should be applied within 1 hour after sanding.
l. Remove masking and protective cover ings.
6-168. 6-178. [RESERVED.] Page 6-36 Par 6-167
SECTION 11. OTHER METALS AND ALLOYS
6-179. NOBLE METAL COATINGS - CLEANUP AND RESTORATION . Silver, platinum, and gold finishes are used in aircraft assemblies because of their resistance to ordi nary surface attack and their improved electri cal or heat conductivity. Silver-plated elec trodes can be cleaned of brown or black sulfide tarnish, by placing them in contact with a piece of magnesium sheet stock while immersed in a warm water solution of common table salt mixed with baking soda or by using a fine grade abrasive mat or pencil eraser followed by solvent cleaning. If assemblies are in volved, careful drying and complete displace ment of water is necessary. In general, clean ing of gold or platinum coatings is not recom mended in the field.
6-180. COPPER AND COPPER ALLOYS are relatively corrosion resistant, and attack on such components will usually be limited to staining and tarnish. Such change in surface condition is not dangerous and should ordinar ily have no effect on the function of the part.
However, if it is necessary to remove such staining, a chromic acid solution of 8 to 24 ounces per gallon of water containing a small amount of battery electrolyte (not to exceed 50 drops per gallon) is an effective brightening bath. Staining may also be removed using a fine grade abrasive mat or pencil eraser fol lowed by solvent cleaning.
a. Immerse the stained part in the cold solution. Surfaces can also be treated in place by applying the solution to the stained surface with a small brush.
b. Avoid any entrapment of the solution after treatment. Clean the part thoroughly following treatment with all residual solution removed.
c. Serious copper corrosion is evident by the accumulation of green-to-blue copper salts on the corroded part. Remove these products mechanically using a stiff bristle brush, brass wire brush, 400-grit abrasive paper or bead blast with glass beads, (specification MIL-G-9954, size 13). Air pressure when blasting should be 20 to 30 psi for direct pres sure machines. Do not bead blast braided cop per flexible lines. Reapply a surface coating over the reworked area. Chromic acid treat ment will tend to remove the residual corro sion products.
WARNING: Brushing, sanding, and abrasive blasting of copper and copper alloys can be dangerous due to the creation of toxic airborne particles.
Take necessary precautions to ensure safety.
6-181. TITANIUM AND TITANIUM AL - LOYS are highly corrosion resistant because an oxide film forms on their surfaces upon contact with air.
a. When titanium is heated, different oxides having different colors form on the sur face. A blue oxide coating will form at 700 to 800 °F; a purple oxide at 800 to 950 °F; and a gray or black oxide at 1000 °F or higher.
These coatings are protective discolorations and should not be removed.
b. Corrosive attack on titanium surfaces is difficult to detect. It may show deterioration from the presence of salt deposits and metal impurities at elevated temperatures so periodic removal of surface deposits is required. How ever, if corrosion develops on titanium, it usu ally occurs as pitting. Acceptable methods for corrosion removal are:
Par 6-179 Page 6-37
(1) Stainless steel wool or hand brush.
(2) Abrasive mats, cloths, and papers with either aluminum oxide or silicon carbide grit.
(3) Dry abrasive blasting using glass beads (spec. MIL-G-9954) sizes 10-13 or Aluminum oxide (spec. MIL-G-21380, type I, grades A or B) at a blast pressure of 40 to 50 psi (if using suction equipment use 50 percent higher pressure).
WARNING: Dry abrasive blasting of titanium alloys creates sparking. Ensure that hazardous concentrations of flammable vapors are not present.
(4) Hand polish with aluminum polish and soft cloth.
c. Titanium surfaces are susceptible to hydrogen embrittlement that can induce stress corrosion and associated pitting. Therefore, chemicals such as fire-resistant hydraulic flu ids must be controlled. Chlorinated hydrocar bon solvents and chemical corrosion removers are prohibited from use on titanium and tita nium alloys.
6-182. 6-192. [RESERVED.] Page 6-38 Par 6-181