used over the heat blanket. This will insulate and prevent damage to the nylon bagging film.
Ensure that the breather plies are in contact with the bleeder plies so that an air passage exists.
(i) Place a bead of sealing tape against the parent material around the edge of the breather plies. Seal the thermocouple wires to prevent vacuum leakage.
NOTE: Two layers of sealing tape may be required in order to provide a good seal.
(j) Cover with a suitable vacuum bag, smoothed to minimize wrinkles. Press the bag firmly onto the sealing tape to obtain an air-tight seal. Place pleats in vacuum bag to allow the bag material to stretch.
(k) Install two vacuum probes or sniffers through openings cut in the bag. One will be used for the vacuum gauge and the other will be connected to the vacuum source.
The vacuum probe must sit on the breather plies, but must not touch the patch or adhesive.
NOTE: Place the vacuum gauge on the opposite side of the vacuum port, where applicable. Do not place vacuum probes near repair area.
(l) Connect the vacuum source and smooth the bag by hand pressure as the air is removed. Check for leaks and reseal as neces sary. A minimum vacuum of 22 inches of mercury is required.
(m) Place insulating material over the vacuum bag to prevent heat loss.
(n) Apply power to the heat blanket and control its temperature as specified for the material being cured.
(o) Observe cure time requirements established by the product manufacturer.
3-5. 3-9. [RESERVED.] Page 3-8 Par 3-4
SECTION 2. METALLIC SANDWICH SECONDARY STRUCTURE REPAIRS
3-10. REPAIRS TO METALLIC SAND- WICH SECONDARY STRUCTURE. Mag nesium, titanium, or stainless steel facings re quire special procedures that are not included in the following methods of repair. Aluminum alloys such as 7075-T6, 2024-T3, and 2014-T6 are commonly used for the repair of facings for sandwich structural parts having aluminum facings. For maximum corrosion resistance, use only clad aluminum for repairs to clad aluminum alloy facings.
a. Dents, scratches, or fractures, not ex ceeding 1/4 inch in largest dimension in alu minum facings, may be repaired with a suit able filler such as viscous epoxy resin. Dents that are delaminated shall not be filled but re paired. Thoroughly clean the repair area with fine sandpaper and acetone before applying the filler. After the resin has partially cured, re move any excess resin with a sharp plastic scraper. When the resin has completely cured, sand to the original contour. If the damage in cluded a fracture, reclean the area around the filled hole and apply a surface patch.
b. Fractures or punctures in one facing and partial damage to the core of an alumi num-faced laminate may be repaired by several different methods. The technique used will depend upon the size of the damage, the strength required, and the aerodynamic loads of the area involved. If the repair requires aerodynamic smoothness, the facing sur rounding the repair core cavity may have to be step cut to one-half its thickness. This can be done by using a router with an end mill bit and a template.
c. Damage that extends completely through the core and both facings may be re paired using the same general techniques as those used for repairing fiberglass laminates when both facings are accessible.
d. After locating the extent of the total damaged area by tapping or other nondestruc tive test methods, remove the damaged facing and that portion of the core material that is also affected. The depth to which the core must be removed will depend upon the type of core material and the method of repair. The re placement core material must be the same material and core cell size as the original. Fab ricate core material to shape, keeping the same core ribbon or grain direction. When a sub stitution is permissible, wood or glass-fabric honey-comb cores are sometimes used in the repair of aluminum honeycomb cores, as they are generally easier to shape. Typical types of core replacements are shown in figure 3-10.
Resin fills can be used to replace the core and facing where smaller core damage exists.
Phenolic microballoons, low-density insulating materials, and/or other ingredients are added to lower the density and give greater flexibility.
e. For the repair of larger holes in which it is inconvenient to use a face patch because of aerodynamic smoothness requirements in that area, both the core and facing are some times replaced with glass-fiber fabric discs and resin. Undercut the core, as shown in fig ure 3-11, in order to obtain a better bonding of the fill with the facing. Fill the core cavity with accurately shaped resin-saturated glass cloth discs, and press each ply down to remove any air bubbles. Special care should be taken that the final plies fit well against the under side of the top facing. When the core cavity is filled, close the cutout in the facing with resinimpregnated glass fiber fabric discs that have been precut to size.
f. Overlap repairs, typically called scab patches, have a long history of use in repairing aircraft structures. These repairs simply cover the damaged area with patch material. Overlap repairs can be bonded and/or mechanically Par 3-10 Page 3-9
A. REPLACEMENT WITH CORE PLUG OF SAME fastened. Figure 3-12 shows a cross-section of
OR OTHER TYPES OF CORE MATERIAL a typical bonded and mechanically fastened re- ORIGINAL CORE PLUG pair. The damaged area may or may not need
HONEYCOMB ROUTED AREA CORE EPOXY-RESIN to be filled.
/ADHESIVE
(1) Bonded overlap repairs work well on most structures. The overlap repair consists B. RESIN FILL of a solid patch material such as metal, pre- EPOXY-RESIN FILL cured laminates, prepreg or wet layup material ORIGINAL PARTIAL OR COMPLETE ROUTED AREA co-cured in place.
HONEYCOMB DEPTH OF CORE CORE
(2) Bolt or blind rivet. Mechanically fastened, bolted, or blind rivet repairs are pri- C. RESIN FILL, UNDERCUT CORE marily used for thick structures. Primary con- ROUTED AREA cerns include bolt/rivet spacing, fastener di- EPOXY-RESIN FILL PARTIAL OR COMPLETE ameter, number of fasteners, and sealant type.
DEPTH OF CORE
ORIGINAL
HONEYCOMB CORE UNDERCUT CORE g. Core potting is the process of filling the core cutout with a curable paste filler material. If the damage is sustained in an area with D. GLASS-CLOTH-RESIN LAMINATE, UNDERCUT CORE an already-potted core, the replacement core GLASS-CLOTH RESIN LAMINATE should also be potted. In other cases, if the ORIGINAL HONEYÇOMB ROUTED ARER honeycomb or foam core is damaged, it may CORE UNDERCUT CORE be potted rather than plugged if the damaged area is small (1 inch or less). Remove the face sheet with a power router, using a router tem- E. REPLACEMENT WITH CORE PLUG OF SAME plate to prevent injury to undamaged face skin.
ORIGINAL TYPE OF SANDWICH CONSTRUCTION COMPLETE SANDWICH ROUTED AREA the face skins only, a face skin and part of the The router may be adjusted to remove one of HONEYCOMB CORE CORE PLUG EPOXY-RESIN ADHESIVE core, a face skin and all of the core, or both the face skins and the core. (See figure 3-13.)
FIGURE 3-10. Typical types of core replacement.
CORE -ORIGINAL CORE TO SKIN ADHESIVE
- JAGGED EDGES
SECTION SHOWING UNDERCUT -FINISHED UNDERCUT AREA FIGURE 3-11. Typical undercut core material cavity.
Page 3-10 Par 3-10
(1) It may be necessary when routing a tapered section such as an aileron to use a wedge-shaped block between the routing tem plate and the upper surface. This will allow the router to cut the core material parallel with the lower surface. (See figure 3-14.)
(2) Select the appropriate potting adhe sive as recommended by the manufacturer.
Mix a sufficient quantity of filler to fill the hole and add microballoons if they are needed to serve as a filler. When the resin and filler are thoroughly mixed according to the manu facturer’s recommendations, pour the mixture into the hole filling all of the cells, then work out all of the bubbles with a toothpick. If per forming an overlay repair fill the core cavity to slightly above the part’s surface. If performing a flush repair, fill the core cavity to slightly above the original core.
(3) Cure the compound according to the manufacturer’s directions. Trim the top of the cured potting compound flush with the surface, for the type of repair you are performing.
h. A core plug repair replaces damaged core material with a shaped piece of similar core material.
(1) Complete removal of core material to the opposite face generally requires some hand-cutting with a core knife. Figure 3-15 shows core material being removed with a core knife. The core can be peeled away from the skin bond using duckbill pliers. Sanding is then required to remove irregular accumula tions of adhesive from the undamaged inner face. Remove only enough adhesive to pro duce a smooth finish.
CAUTION: Care should be used when peeling core material from thinskin sandwich face sheets, because the skin can be damaged by pulling on the core.
FIGURE 3-12. Cross section of bonded and bolted over lap repairs.
FIGURE 3-13. Honeycomb core removal.
FIGURE 3.14 Removing honeycomb core from a tapered control surface.
FIGURE 3-15. Removal of core with core knife.
Par 3-10 Page 3-11
(2) A core plug should be fabricated as follows. Select the core density. Cell size and ribbon direction and thickness should be at least the same as that used in the original con struction. Trim the sides of the plug to a loose fit in the routed cavity. Trim the plug height so the top of the plug sits .001 inch higher than the level of the original surface. The core will compress and set during cure thereby requiring the extra height. Carefully remove the trimmed core plug from the machined cavity.
Use a vacuum cleaning device to remove any dust or particles remaining on the core plug or in the repair area. Clean the core plug by rinsing with an approved solvent and wrap the plug in a clean polyethylene bag until needed for assembly.
CAUTION: When handling film ad - hesives, prepreg fabrics, or parts with prepared surfaces, latex gloves must be worn.
(3) Using a film adhesive, the core plug should be installed as follows. Select the ap propriate adhesive film. Cut one disk of adhe sive to the same shape and size as the perime ter of the repair cutout if the repair extends through the entire core thickness. Cut two disks if a partial depth core repair is being made. Cut one strip of core splice adhesive to wrap around the core perimeter to its full depth. For a partial depth core repair, also cut out a fiberglass or aluminum disk, again matching the size and the shape of the repair cutout. Figure 3-16 shows the details of a par tial depth core repair. Preassemble the pieces.
(4) Wipe the bottom and sides of the cutout area with solvent. Allow the area to dry. Insert the core plug assembly with splice adhesive applied to the perimeter into the core cutout. Ensure the core plug ribbon direction matches that of the parent core. In the case of a partial depth core repair, the plug and disk FIGURE 3-16. Details of core repair.
may be cured to save time. Some restraining method, such as vacuum bagging, may be de sirable over the core splice adhesive as this material usually foams up and out during cure.
Cure the adhesive according to the manufac turer’s directions and allow the area to cool.
(5) Trim the top of the cured core plug flush with either the original core or the mold line, depending on the type of laminate repair to be performed. Proceed with laminate repair.
3-11. FINISHING. The type of finish coating applied to a metallic sandwich repair will normally be determined by the exposed material and the application of the part or as sembly. Rain erosion of plastic parts, the need for electrical or dielectric properties, and/or the necessity for anti-corrosion coatings must be considered when the choice of finish is made.
Plastic-faced parts such as radomes are fin ished primarily for rain erosion while alumi num- or other metal-faced laminates are Page 3-12 Par 3-10
finished for corrosion protection. For coatings to perform their function properly, it is essen tial that they be applied to surfaces that are clean, free of voids, and smooth. The edges of all parts not protected by a bonding of alumi num or glass-fabric laminate must be sealed to reduce the rate of moisture absorption.
3-12. 3-17. [RESERVED.] Par 3-11 Page 3-13 (and 3-14)
SECTION 3. TRANSPARENT PLASTICS
3-18. GENERAL. Plastics cover a broad field of organic synthetic resin and may be di vided into two main classifications – thermo plastics and thermosetting plastics.
a. Thermoplastics. Thermoplastics may be softened by heat and can be dissolved in various organic solvents. Two kinds of trans parent thermoplastic materials are commonly employed in windows, canopies, etc. These materials are known as acrylic plastics and cellulose acetate plastics.
(1) Cellulose acetate was used in the past but since it is dimensionally unstable and turns yellow after it has been installed for a time, it has just about passed from the scene and is not considered an acceptable substitute for acrylic.
(2) Acrylic plastics are known by the trade names of Lucite or Plexiglas and by the British as Perspex and meet the military speci fications of MIL-P-5425 for regular acrylic, MIL-P-8184 for craze-resistant acrylic.
b. Thermosetting Plastics. These plas tics do not soften appreciably under heat but may char and blister at temperatures of 240 to 260 °C (400 to 500 °F). Most of the molded products of synthetic resin composi tion, such as phenolic, urea-formaldehyde, and melamine formaldehyde resins, belong to the thermosetting group. Once the plastic be comes hard, additional heat will not change it back into a liquid as it would with a thermo plastic.
3-19. STORAGE AND HANDLING. Be cause transparent thermoplastic sheets soften and deform when they are heated, they must be stored where the temperature will never be come excessive. Store them in a cool, dry location away from heating coils, radiators, or steam pipes, and away from such fumes as are found in paint spray booths or paint storage ar eas.
a. Paper-masked transparent sheets must be kept out of the direct rays of the sun, because sunlight will accelerate deterioration of the adhesive, causing it to bond to the plas tic and making it difficult to remove.
b. Plastic sheets should be stored with the masking paper in place, in bins that are tilted at a ten-degree angle from the vertical. This will prevent their buckling. If the sheets are stored horizontally, take care to avoid getting dirt and chips between them. Stacks of sheets must never be over 18 inches high, with the smallest sheets stacked on top of the larger ones so there will be no unsupported overhang.
Leave the masking paper on the sheets as long as possible, and take care not to scratch or gouge the sheets by sliding them against each other or across rough or dirty tables.
c. Formed sections should be stored with ample support so they will not lose their shape.
Vertical nesting should be avoided. Protect formed parts from temperatures higher than 120 °F (49 °C), and leave their protective coating in place until they are installed on the aircraft.
3-20. FORMING PROCEDURES AND TECHNIQUES. Transparent acrylic plastics get soft and pliable when they are heated to their forming temperatures and can be formed to almost any shape. When they cool, they re tain the shape to which they were formed.
Acrylic plastic may be cold-bent into a single curvature if the material is thin and the bend ing radius is at least 180 times the thickness of the sheet. Cold bending beyond these limits Par 3-18 Page 3-15
will impose so much stress on the surface of the plastic that tiny fissures or cracks, called crazing, will form.
3-21. HEATING. Before heating any trans parent plastic material, remove all of the masking paper and adhesive from the sheet. If the sheet is dusty or dirty, wash it with clean water and rinse it well. Dry the sheet thor oughly by blotting it with soft absorbent paper towels.
NOTE: Wear cotton gloves when handling the plastic to eliminate finger marks on the soft surface.
a. For the best results when hot-forming acrylics, use the temperatures recommended by the manufacturer. A forced-air oven should be used −one that is ca pable of operating over a temperature range of 120 to 374 °F (49 to 190 °C). If the part gets too hot during the forming process, bubbles may form on the surface and impair the optical qualities of the sheet.
b. For uniform heating, it is best to hang the sheets vertically by grasping them by their edges with spring clips and suspending the clips in a rack. (See figure 3-17.) If the piece is too small to hold with clips, or if there is not enough trim area, lay the sheets on shelves or racks covered with soft felt or flannel. Be sure there is enough open space to allow the air to circulate around the sheet and heat it evenly.
c. Small forming jobs, such as landing light covers, may be heated in a kitchen baking oven. Infrared heat lamps may be used if they are arranged on 7-or 8-inch centers and enough of them are used in a bank to heat the sheet evenly. Place the lamps about 18 inches from the material.
FIGURE 3-17. Hanging of acrylic sheets.
d. Never use hot water or steam directly on the plastic to heat it, because this will likely cause the acrylic to become milky or cloudy.
3-22. FORMS. Heated acrylic plastic will mold with almost no pressure, so the forms used can be of very simple construction.
Forms made of pressed wood, plywood, or plaster are adequate to form simple curves, but reinforced plastic or plaster may be needed to shape complex or compound curves.
a. Since hot plastic conforms to any waviness or unevenness, the form used must be completely smooth. To ensure this, sand the form and cover it with soft cloth such as outing flannel or billiard felt.
b. The mold should be large enough to extend beyond the trim line of the part, and provisions should be made for holding the hot plastic snug against the mold as it cools.
c. A mold can be made for a complex part by using the damaged part itself. If the part is broken, tape the pieces together, wax or grease the inside so the plaster will not stick to it, and support the entire part in sand. Fill the part with plaster and allow it to harden, and Page 3-16 Par 3-20
then remove it from the mold. Smooth out any roughness and cover it with soft cloth. It is now ready to use to form the new part.
3-23. FORMING METHODS. (See ta ble 3-1.)
a. Simple Curve Forming. Heat the plastic material to the recommended tempera ture, remove it from the heat source, and care fully drape it over the prepared form. Care fully press the hot plastic to the form and ei ther hold or clamp the sheet in place until it cools. This process may take from ten minutes to one-half hour. Do not force-cool it.
b. Compound-Curve Forming. This type of forming is normally used for such parts as canopies or complex wingtip light covers, and it requires a great deal of specialized equipment. There are four commonly used methods, each having its advantages and dis advantages.
c. Stretch Forming. Preheated acrylic sheets are stretched mechanically over the form in much the same way as is done with the simple curved piece. Special care must be taken to preserve uniform thickness of the material, since some parts will have to stretch more than others.
d. Male And Female Die Forming. This requires expensive matching male and female dies. The heated plastic sheet is placed be tween the dies which are then mated. When the plastic cools, the dies are opened.
e. Vacuum-Forming Without Forms.
Many aircraft canopies are formed by this method. In this process a clamp with an opening of the desired shape is placed over a vacuum box and the heated sheet of plastic is clamped in place. When the air in the box is evacuated, the outside air pressure will force the hot plastic through the opening and form the concave canopy. It is the surface tension of the plastic that shapes the canopy.
f. Vacuum-Forming With A Female Form. If the shape needed is other than that which would be formed by surface tension, a female mold, or form must be used. It is placed below the plastic sheet and the vacuum pump is connected. When air from the form is evacuated, the outside air pressure will force the hot plastic sheet into the mold and fill it.
g. Sawing And Drilling.
(1) Several types of saws can be used with transparent plastics, however circular saws are the best for straight cuts. The blades TABLE 3-1. Typical temperatures for forming acrylic sheets.
Thickness of sheet (in.) 0.125 0.250 0.125 0.250 Type of forming Regular acrylic plastic.
MIL-P-6886 Heat-resistant acrylic plastic, MIL-P-5425, and craze-resistant acrylic plastic, MIL-P-8184 °C °F °C °F °C °F °C °F Simple curve 113 235 110 230 135 275 135 275 Stretch forming (dry mold cover) 140 284 135 275 160 320 150 302 Male and female forming 140 284 135 275 180 356 170 338 Vacuum forming without form 140 284 135 275 150 302 145 293 Vacuum forming with female form 145 293 140 284 180 356 170 338 Par 3-22 Page 3-17
should be hollow -ground or have some set to prevent binding. After the teeth are set, they should be side -dressed to produce a smooth edge on the cut. Band saws are recommended for cutting flat acrylic sheets when the cuts must be curved or where the sheet is cut to a rough dimension to be trimmed later. Close control of size and shape may be obtained by band sawing a piece to within 1/16 inch of the desired size, as marked by a scribed line on the plastic, and then sanding it to the correct size with a drum or belt sander.
(2) Unlike soft metal, acrylic plastic is a very poor conductor of heat. Make provisions for removing the heat when drilling. Deep holes need cooling, and a water-soluble cutting oil is a satisfactory coolant since it has no ten dency to attack the plastic.
(a) The drill used on acrylics must be carefully ground and free from nicks and burrs that would affect the surface finish. Grind the drill with a greater included angle than would be used for soft metal. The rake angle should be zero in order to scrape, not cut. (See fig ure 3-18.)
FIGURE 3-18. Drill having an included angle of approximately 150°, used to drill acrylic plastics.
(b) The patented Unibit (see fig ure 3-19) is good for drilling small holes in aircraft windshields and windows. It can cut holes from 1/8-to 1/2 −inch in 1/32 −inch in crements and produces good smooth holes with no stress cracks around their edges.
FIGURE 3-19. Unibit drill for drilling acrylic plastics.
h. Polymerizable Cements. Polymeri zable cements are those in which a catalyst is added to an already thick monomerpolymer syrup to promote rapid hardening. Ce ment PS-30 and Weld -On 40 are polymeri zable cements of this type. They are suitable for cementing all types of PLEXIGLAS acrylic cast sheet and parts molded from PLEXIGLAS molding pellets. At room temperature, the cements harden (polymerize) in the container in about 45 minutes after mixing the compo nents. They will harden more rapidly at higher temperatures. The cement joints are usually hard enough for handling within 4 hours after assembly. The joints may be machined within 4 hours after assembly, but it is better to wait 24 hours.
(1) PS-30 and Weld -On 40 joints retain excellent appearance and color stability after outdoor exposure. These cements produce clear, transparent joints and should be used when the color and appearance of the joints are important.
(2) PS-30 and Weld -On 40 should be used at temperatures no lower than 65 °F. If cementing is done in a room cooler than 65 °F, it will require a longer time to harden and the joint strength will be reduced.
(a) The cement should be prepared with the correct proportions of components as given in the manufacturer’s instructions and thoroughly mixed, making sure neither the mixing container nor mixing paddle adds color or affects the hardening of the cement.
Page 3-18 Par 3-23
Clean glass or polyethylene mixing containers are preferred.
(b) Because of their short pot life (approximately 45 minutes) Cement PS-30 and Weld-On 40 must be used quickly once the components are mixed. Time consumed in preparation shortens the effective working time, making it necessary to have everything ready to be cemented before the cements are mixed. For better handling pour cement within 20 minutes of mixing.
(c) For maximum joint strength, the final cement joint should be free of bubbles. It will usually be sufficient to allow the mixed cement to stand for 10 minutes before ce menting to allow bubbles to rise to the surface.
(See figure 3-20.)
FIGURE 3-20. Applying pressure to acrylic plastics.
(d) The gap joint technique can only be used with colorless PLEXIGLAS acrylic or in cases in which joints will be hidden. If in conspicuous joints in colored PLEXIGLAS acrylic are needed, the parts must be fitted closely, using closed V groove, butt, or arc joints.
(3) Cement forms or dams may be made with masking tape as long as the adhesive sur face does not contact the cement. This is easily done with a strip of cellophane tape placed over the masking tape adhesive. The tape must be chosen carefully. The adhesive on ordinary cellophane tape prevents the cure of PS-30 and Weld-On 40. Before actual fab rication of parts, sample joints should be tried to ensure that the tape system used will not harm the cement. Since it is important for all of the cement to remain in the gap, only con tact pressure should be used.
(4) Bubbles will tend to float to the top of the cement bead in a gap joint after the ce ment is poured. These cause no problem if the bead is machined off. A small wire (not cop per), or similar objects may be used to lift some bubbles out of the joint; however, the cement joint should be disturbed as little as possible.
(5) Polymerizable cements shrink as the cement hardens. Therefore, the freshly poured cement bead should be left above the surfaces being cemented to compensate for the shrink age. If it is necessary for appearances, the bead may be machined off after the cement has set.
3-24. REPAIR OF PLASTICS. Replace, rather than repair extensively damaged trans parent plastic, whenever possible, since even a carefully patched part is not the equal of a new section, either optically or structurally. At the first sign of crack development, drill a small hole with a # 30 or a 1/8-inch drill at the ex treme ends of the cracks as shown in fig ure 3-21. This serves to localize the cracks and to prevent further splitting by distributing the strain over a large area. If the cracks are small, stopping them with drilled holes will usually suffice until replacement or more per manent repairs can be made. The following repairs are permissible; however, they are not to be located in the pilot’s line of vision during landing or normal flight.
Par 3-23 Page 3-19
ALL THE STRAINS WHICH ORIGINALLY CAUSED
THE CRACK ARE CONCENTRATED AT POINT A - TENDING TO EXTEND THE CRACK. THEREFORE DRILL, WITH A #30 OR 1/8" DRILL BIT, A SMALL HOLE AT END OF THE CRACK POINT A1) TO DISTRIBUTE THE STRAIN OVER A WIDER AREA.
EACH CRACK OCCURRING AT ANY HOLE OR TEAR IS DRILLED IN SAME MANNER.
FIGURE 3-21. Stop-drilling cracks.
a. Surface Patch. If a surface patch is to be installed, trim away the damaged area and RFACE PATCI round all corners. Cut a piece of plastic of sufficient size to cover the damaged area and ex- STOP CRÁCK DRILLED tend at least 3/4 inch on each side of the crack or hole. Bevel the edges as shown in figure 3-22. If the section to be repaired is SURFACE PATCH FOR CRACKS BEVELED EDGE curved, shape the patch to the same contour by heating it in an oil bath at a temperature of IRFACE PATCH 248 to 302 °F, or it may be heated on a TRIM DAMAGED AREA AND ROUND ALL CORNERS hot-plate until soft. Boiling water should not CORNER HARP be used for heating. Coat the patch evenly with plastic solvent adhesive and immediately place it over the hole. Maintain a uniform SURFACE PATCH FOR IRREGULAR SHAPED DAMAGE / 'EDGE BEVELED pressure of 5 to 10 psi on the patch for a minimum of 3 hours. Allow the patch to dry 24 to 36 hours before sanding or polishing.
ROUI
b. Plug Patch. When using inserted patches to repair holes in plastic structures, BEVELED EDGE trim the holes to a perfect circle or oval and SURFACE PATCH FOR ROUND HOLES ' bevel the edges slightly. Make the patch slightly thicker than the material being FIGURE 3-22. Surface patches.
Page 3-20 Par 3-24