AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 124–135
Page 136Open in PDF

repaired and similarly bevel its edges. Install patches in accordance with figure 3-23. Heat the plug until soft and press it into the hole without cement and allow to cool to make a perfect fit. Remove the plug, coat the edges with adhesive, and then reinsert in the hole.

Maintain a firm light pressure until the cement has set. Sand or file the edges level with the surface, then buff and polish.

FIGURE 3-23. Plug patch repair.

3-25. CLEANING AND POLISHING TRANSPARENT PLASTIC. Plastics have many advantages over glass for aircraft use, but they lack the surface hardness of glass and care must be exercised while servicing the air­ craft to avoid scratching or otherwise damag­ ing the surface.

a. Clean the plastic by washing it with plenty of water and mild soap, using a clean, soft, grit-free cloth, sponge, or bare hands. Do not use gasoline, alcohol, benzene, acetone, carbon tetrachloride, fire extinguisher or deic­ ing fluids, lacquer thinners, or window clean­ ing sprays. These will soften the plastic and cause crazing.

b. Plastics should not be rubbed with a dry cloth since this is likely to cause scratches, and also to build up an electrostatic charge that attracts dust particles to the surface. If after removing dirt and grease, no great amount of scratching is visible, finish the plastic with a good grade of commercial wax. Apply the wax in a thin even coat and bring to a high polish by rubbing lightly with a soft cloth.

c. Do not attempt hand polishing or buffing until the surface is clean. A soft, open-type cotton or flannel buffing wheel is suggested. Minor scratches may be removed by vigorously rubbing the affected area by hand, using a soft clean cloth dampened with a mixture of turpentine and chalk, or by applying automobile cleanser with a damp cloth. Re­ move the cleaner and polish with a soft, dry cloth. Acrylic and cellulose acetate plastics are thermoplastic. Friction created by buffing or polishing too long in one spot can generate sufficient heat to soften the surface. This con­ dition will produce visual distortion and should be avoided.

3-26. REPLACEMENT PANELS. Use material equivalent to that originally used by the manufacturer of the aircraft for replace­ ment panels. There are many types of trans­ parent plastics on the market. Their properties vary greatly, particularly in regard to expan­ sion characteristics, brittleness under low Par 3-24 Page 3-21

Page 137Open in PDF

temperatures, resistance to discoloration when exposed to sunlight, surface checking, etc. In­ formation on these properties is in MIL-HDBK-17A, Plastics for Flight Vehicles, Part IITransparent Glazing Materials, avail­ able from the Government Printing Office (GPO). These properties are considered by aircraft manufacturers in selecting materials to be used in their designs and the use of substi­ tutes having different characteristics may result in subsequent difficulties.

3-27. INSTALLATION PROCEDURES.

When installing a replacement panel, use the same mounting method employed by the manufacturer of the aircraft. While the actual installation will vary from one type of aircraft to another, consider the following major prin­ ciples when installing any replacement panel.

a. Never force a plastic panel out of shape to make it fit a frame. If a replacement panel does not fit easily into the mounting, obtain a new replacement or heat the whole panel and reform. When possible, cut and fit a new panel at ordinary room temperature.

b. In clamping or bolting plastic panels into their mountings, do not place the plastic under excessive compressive stress. It is easy to develop more than 1,000 psi on the plastic by over-torquing a nut and bolt. Tighten each nut to a firm fit, then back the nut off one full turn (until they are snug and can still be rotated with the fingers).

c. In bolted installations, use spacers, collars, shoulders, or stop-nuts to prevent tightening the bolt excessively. Whenever such devices are used by the aircraft manufac­ turer, retain them in the replacement installa­ tion. It is important that the original number of bolts, complete with washers, spacers, etc., be used. When rivets are used, provide ade­ quate spacers or other satisfactory means to prevent excessive tightening of the frame to the plastic.

d. Mount plastic panels between rubber, cork, or other gasket material to make the in­ stallation waterproof, to reduce vibration, and to help to distribute compressive stresses on the plastic.

e. Plastics expand and contract consid­ erably more than the metal channels in which they are mounted. Mount windshield panels to a sufficient depth in the channel to prevent it from falling out when the panel contracts at low temperatures or deforms under load.

When the manufacturer’s original design per­ mits, mount panels to a minimum depth of 1-1/8 inch, and with a clearance of 1/8 inch between the plastic and bottom of the channel.

f. In installations involving bolts or rivets, make the holes through the plastic over­ size by 1/8-inch diameter and center so that the plastic will not bind or crack at the edge of the holes. The use of slotted holes is also recom­ mended.

3-28.  3-39. [RESERVED.] Page 3-22 Par 3-26

Page 138Open in PDF

SECTION 4. WINDSHIELDS, ENCLOSURES, AND WINDOWS

3-40. GENERAL. These repairs are appli­ cable to plastic windshields, enclosures, and windows in nonpressurized airplanes . For pressurized airplanes, replace or repair plastic elements in accordance with the manufac­ turer’s recommendation. When windshields and side windows made of acrylic plastics are damaged, they are usually replaced unless the damage is minor and a repair would not be in the line of vision. Repairs usually require a great deal of labor. Replacement parts are readily available, so replacement is normally more economical than repair.

a. Minor Repairs. There are times, how­ ever, when a windshield may be cracked and safety is not impaired. In that case, repairs can be made by stop-drilling the ends of the crack with a # 30 drill (1/8 inch) to prevent the con­ centration of stresses causing the crack to con­ tinue. Drill a series of number 40 holes a half-inch from the edge of the crack about a half-inch apart, and lace through these holes with brass safety wire (see figure 3-24) and seal with clear silicone to waterproof.

b. Temporary Repairs. One way to make a temporary repair is to stop-drill the ends of the crack, and then drill number 27 holes every inch or so in the crack. Use AN515-6 screws and AN365-632 nuts with AN960-6 washers on both sides of the plastic.

This will hold the crack together and prevent further breakage until the windshield can be properly repaired or replaced. (See fig­ ure 3-24.)

c. Permanent Repairs. Windshields or side windows with small cracks that affect only the appearance rather than the airworthi­ ness of a sheet, may be repaired by first stop-drilling the ends of the crack with a # 30 or a 1/8-inch drill. Then use a hypoder­ mic syringe and needle to fill the crack with polymerizable cement such as PS-30 or Weld-On 40, and allow capillary action to fill the crack completely. Soak the end of a 1/8-inch acrylic rod in cement to form a cush­ ion and insert it in the stop-drilled hole. Allow the repair to dry for about 30 minutes, and then trim the rod off flush with the sheet.

d. Polishing and Finishing. Scratches and repair marks, within certain limitations, can be removed from acrylic plastic. No sanding that could adversely affect the plas­ tic’s optical properties and distort the pilot’s vision should be done on any portion of a windshield.

(1) If there are scratches or repair marks in an area that can be sanded, they may be re­ moved by first sanding the area. Use 320- or 400-grit abrasive paper that is wrapped around a felt or rubber pad.

(2) Use circular rubbing motions, light pressure, and a mild liquid soap solution as a lubricant. After the sanding is complete, rinse the surface thoroughly with running water.

Then, using a 500-grit paper, continue to sand lightly. Keep moving to higher grit paper and sand and rinse until all of the sanding or repair marks have been removed.

(3) After using the finest abrasive pa­ per, use rubbing compound and buff in a cir­ cular motion to remove all traces of the sand­ ing.

e. Cleaning. Acrylic windshields and windows may be cleaned by washing them with mild soap and running water. Rub the surface with your bare hands in a stream of water. Follow with the same procedure but with soap and water. After the soap and dirt have been flushed away, dry the surface with a soft, clean cloth or tissue and polish it with a Par 3-40 Page 3-23

Page 139Open in PDF

FIGURE 3-24. Temporary repairs to cracked windshields or windows.

windshield cleaner especially approved for use on aircraft transparent plastics. These cleaners may be purchased through aircraft supply houses.

f. Waxing. A thin coating of wax will fill any minute scratches that may be present and will cause rain to form droplets that are easily blown away by the wind.

3-41. PROTECTION. Acrylic windshields are often called “lifetime” windshields, to dis­ tinguish them from those made of the much shorter-lived acetate material. However, even acrylic must be protected from the ravages of the elements.

a. When an aircraft is parked in direct sunlight, the windshield will absorb heat and will actually become hotter than either the in­ side of the aircraft or the outside air. The sun will cause the inside of a closed aircraft to be­ come extremely hot, and this heat is also ab­ sorbed by the plastic windshield.

b. To protect against this damage, it is wise to keep the aircraft in a hangar. If this is not possible, some type of shade should be provided to keep the sun from coming in direct contact with the windshield. Some aircraft owners use a close-fitting, opaque, reflective cover over the windshield. In many cases, this has done more harm than good. This cover may absorb moisture from the air and give off harmful vapors, and if it touches the surface of the plastic it can cause crazing or minute cracks to form in the windshield. Another hazard in using such a cover is that sand can blow up under the cover and scratch the plas­ tic.

3-42. WINDSHIELD INSTALLATION.

Aircraft windshields may be purchased either from the original aircraft manufacturer or from any of several FAA-PMA sources. These windshields are formed to the exact shape re­ quired, but are slightly larger than necessary so they may be trimmed to the exact size.

a. After removing the damaged windshield, clean all of the sealer from the grooves and cut the new windshield to fit. New wind­ shields are covered with either protective paper or film to prevent damage during handling or installation. Carefully peel back just enough of this covering to make the installation. The windshield must fit in its channels with about 1/8- to 1/4-inch clearance to allow for expan­ sion and contraction. If any holes are drilled in the plastic for screws, they should be about 1/8 inch oversize.

Page 3-24 Par 3-40

Page 140Open in PDF

b. Place the sealing tape around the edges of the windshield and install the wind­ shield in its frame. Screws that go through the windshield should be tightened down snug and then backed out a full turn, so the plastic can shift as it expands and contracts.

c. Do not remove the protective paper or film until the windshield is installed and all of the securing screws are in place.

3-43.  3-47. [RESERVED.] Par 3-42 Page 3-25 (and 3-26)

Page 141Open in PDF

CHAPTER 4. METAL STRUCTURE, WELDING, AND BRAZING

SECTION 1. IDENTIFICATION OF METALS

4-1. GENERAL. Proper identification of the aircraft structural material is the first step in ensuring that the continuing airworthiness of the aircraft will not be degraded by making an improper repair using the wrong materials.

a. Ferrous (iron) alloy materials are generally classified according to carbon con­ tent. (See table 4-1.)

TABLE 4-1. Ferrous (iron) alloy materials.

MATERIALS CARBON CONTENT Wrought iron Trace to 0.08% Low carbon steel 0.08% to 0.30% Medium carbon steel 0.30% to 0.60% High carbon steel 0.60% to 2.2% Cast iron 2.3% to 4.5%

b. The strength and ductility, or tough­ ness of steel, is controlled by the kind and quantity of alloys used and also by cold-working or heat-treating processes used in manufacturing. In general, any process that increases the strength of a material will also decrease its ductility.

c. Normalizing is heating steel to ap­ proximately 150 °F to 225 °F above the steel’s critical temperature range, followed by cooling to below that range in still air at ordinary tem­ perature. Normalizing may be classified as a form of annealing. This process also removes stresses due to machining, forging, bending, and welding. After the metal has been held at this temperature for a sufficient time to be heated uniformly throughout, remove the metal from the furnace and cool in still air. Avoid prolonging the soaking of the metal at high temperatures, as this practice will cause the grain structure to enlarge. The length of time required for the soaking temperature de­ pends on the mass of the metal being treated.

The soaking time is roughly ¼ hour per inch of the diameter of thickness (Ref: Military Tech Order (T.O.) 1-1A-9).

4-2. IDENTIFICATION OF STEEL STOCK. The Society of Automotive Engi­ neers (SAE) and the American Iron and Steel Institute (AISI) use a numerical index system to identify the composition of various steels.

The numbers assigned in the combined listing of standard steels issued by these groups repre­ sent the type of steel and make it possible to readily identify the principal elements in the material.

a. The basic numbers for the four digit series of the carbon and alloy steel may be found in table 4-2. The first digit of the four number designation indicates the type to which the steel belongs. Thus, “1” indicates a carbon steel, “2” a nickel steel, “3” a nickel chromium steel, etc. In the case of simple alloy steels, the second digit indicates the approximate per­ centage of the predominant alloying element.

The last two digits usually indicate the mean of the range of carbon content. Thus, the desig­ nation “1020” indicates a plain carbon steel lacking a principal alloying element and con­ taining an average of 0.20 percent

(0.18 to 0.23) carbon. The designation “2330” indicates a nickel steel of approximately 3 percent (3.25 to 3.75) nickel and an average of 0.30 percent, (0.28 to 0.33) carbon content.

The designation “4130” indicates a chromiummolybdenum steel of approximately 1 percent

(0.80 to 1.10) chromium, 0.20 percent

(0.15 to 0.25) molybdenum, and 0.30 percent

(0.28 to 0.33) carbon.

Par 4-5 Page 4-1

Page 142Open in PDF

b. There are numerous steels with higher percentages of alloying elements that do not fit into this numbering system. These include a large group of stainless and heat resisting al­ loys in which chromium is an essential alloy­ ing element. Some of these alloys are identi­ fied by three digit AISI numbers and many others by designations assigned by the steel company that produces them. The few exam­ ples in table 4-3 will serve to illustrate the kinds of designations used and the general al­ loy content of these steels.

c. “1025” welded tubing as per Specification MIL-T-5066 and “1025” seamless tubing con­ forming to Specification MIL-T-5066A are inter­ changeable.

4-3. INTERCHANGEABILITY OF STEEL TUBING .

a. “4130” welded tubing conforming to Specification MIL-T-6731, and “4130” seam-less tubing conforming to Specification MIL-T-6736 are interchangeable.

b. NE-8630 welded tubing conforming to Specification MIL -T-6734, and NE- 8630 seamless tubing conforming to Specification MIL-T-6732 are interchangeable.

4-4. IDENTIFICATION OF ALUMINUM .

To provide a visual means for identifying the various grades of aluminum and aluminum alloys, such metals are usually marked with symbols such as a Government Specification Number, the temper or condition furnished, or the commercial code marking. Plate and sheet are usually marked with specification numbers or code markings in rows approximately 5 inches apart. Tubes, bars, rods, and extruded shapes are marked with specification numbers or code markings at intervals of 3 to 5 feet along the length of each piece.

The commercial code marking consists of a number which identifies the particular compo­ sition of the alloy. In addition, letter suffixes (see table 4-4) designate the basic temper des­ ignations and subdivisions of aluminum alloys.

TABLE 4-2. Numerical system for steel identification.

TYPES OF STEELS NUMERALS

AND DIGITS Plain carbon steel 10XX Carbon steel with additional sulfur for easy machining.

11XX Carbon steel with about 1.75% manganese 13XX .25% molybdenum. 40XX 1% chromium, .25% molybdenum 41XX 2% nickel, 1% chromium, .25% molybdenum 43XX

1.7% nickel, .2% molybdenum 46XX

3.5% nickel, .25% molybdenum 48XX 1% chromium steels 51XX 1% chromium, 1.00% carbon 51XXX

1.5% chromium steels 52XX

1.5% chromium, 1.00% carbon 52XXX 1% chromium steel with .15% vanadium 61XX .5% chromium, .5% nickel, .20% molybdenum 86XX .5% chromium, .5% nickel, .25% molybdenum 87XX 2% silicon steels, .85% manganese 92XX

3.25% nickel, 1.20% chromium, .12% molybdenum 93XX Page 4-2 Par 4-2

Page 143Open in PDF

TABLE 4-3. Examples of stainless and heat-resistant steels nominal composition (percent)

ALLOY DESIGNATION CARBON CHROMIUM NICKEL OTHER GENERAL CLASS OF STEEL 302 0.15 18 9 Austenitic 310 0.25 25 20 Austenitic 321 0.08 18 11 Titanium Austenitic 347 0.08 18 11 Columbium or Tantalum Austenitic 410 0.15 12.5 Martensitic, Magnetic 430 0.12 17 Ferritic, Magnetic 446 0.20 25 Nitrogen Ferritic, Magnetic PH15-7 Mo 0.09 15 7 Molybdenum, Aluminum Precipitation Hardening 17-4 PH 0.07 16.5 4 Copper, Columbium or Tantalum Precipitation Hardening Par 4-5 Page 4-3

Page 144Open in PDF

TABLE 4-4. Basic temper designations and subdivisions from aluminum alloys.

NON HEAT-TREATABLE ALLOYS HEAT-TREATABLE ALLOYS Temper Designation Definition Temper Designation Definition -0 Annealed recrystallized (wrought products only) applies to softest temper of wrought products.

-0 Annealed recrystallized (wrought products only) applies to softest temper of wrought products.

-H1 Strain-hardened only. Applies to products which are strain-hardened to obtain the desired strength without supplementary thermal treatment.

-T1 Cooled from an elevated temperature shaping process (such as extrusion or casting) and naturally aged to a substantially stable condition.

-H12 Strain-hardened one-quarter-hard temper. -T2 Annealed (castings only).

-H14 Strain-hardened half-hard temper. -T3 Solution heat-treated and cold-worked by the flattening or straightening operation.

-H16 Strain-hardened three-quarters-hard temper. -T36 Solution heat-treated and cold-worked by reduction of 6 percent -H18 Strain-hardened full-hard temper. -T4 Solution heat-treated.

-H2 Strain-hardened and then partially annealed. Applies to products which are strain-hardened more than the desired final amount and then reduced in strength to the desired level by partial annealing.

-T42 Solution heat-treated by the user regardless of prior temper (applicable only to 2014 and 2024 alloys).

-H22 Strain-hardened and partially annealed to one-quarter-hard temper.

-T5 Artificially aged only (castings only).

-H24 Strain-hardened and partially annealed to half-hard temper.

-T6 Solution heat-treated and artificially aged.

-H26 Strain-hardened and partially annealed to three-quarters-hard temper.

-T62 Solution heat-treated and aged by user regardless of prior temper (applicable only to 2014 and 2024 alloys).

-H28 Strain-hardened and partially annealed to full-hard temper.

-T351, -T451, -T3510, -T3511, -T4510, -T4511.

Solution heat-treated and stress relieved by stretching to produce a permanent set of 1 to 3 percent, depending on the product.

-H3 Strain-hardened and then stabilized. Applies to products which are strain-hardened and then stabilized by a low temperature heating to slightly lower their strength and increase ductility.

-T651, -T851, -T6510, -T8510, -T6511, -T8511.

Solution heat-treated, stress relieved by stretching to produce a permanent set of 1 to 3 percent, and artificially aged.

-H32 Strain-hardened and then stabilized. Final temper is one-quarter hard.

-T652 Solution heat-treated, compressed to produce a permanent set and then artificially aged.

-H34 Strain-hardened and then stabilized. Final temper is one-half hard.

-T8 Solution heat-treated, cold-worked and then artificially aged.

-H36 Strain-hardened and then stabilized. Final temper is three-quarters hard.

-T/4 Solution heat-treated, cold-worked by the flattening or straightening operation, and then artificially aged.

-H38 Strain-hardened and then stabilized. Final temper is full-hard.

-T86 Solution heat-treated, cold-worked by reduction of 6 percent, and then artificially aged.

-H112 As fabricated; with specified mechanical property limits.

-T9 Solution heat-treated, artificially aged and then cold-worked.

-F For wrought alloys; as fabricated. No mechanical properties limits. For cast alloys; as cast.

-T10 Cooled from an elevated temperature shaping process artificially aged and then cold-worked.

-F For wrought alloys; as fabricated. No mechanical properties limits. For cast alloys; as cast.

4-5. - 4-15. [RESERVED.] Page 4-4 Par 4-2

Page 145Open in PDF

SECTION 2. TESTING OF METALS

4-16. HARDNESS TESTING . If the mate­ rial type is known, a hardness test is a simple way to verify that the part has been properly heat-treated. Hardness testers such as Rock­ well, Brinell, and Vickers can be useful to check metals for loss of strength due to expo­ sure to fire or abusive heating. Also, under­ strength bolts can be found and removed from the replacement part inventory by checking the hardness of the bolt across the hex flats. Al­ though hardness tests are generally considered nondestructive, hardness testing does leave a small pit in the surface; therefore, hardness tests should not be used on sealing surfaces, fatigue critical parts, load bearing areas, etc., that will be returned to service. These hard­ ness tests provide a convenient means for de­ termining, within reasonable limits, the tensile strength of steel. It has several limitations in that it is not suitable for very soft or very hard steels. Hardness testing of aluminum alloys should be limited to distinguishing between annealed and heat-treated material of the same aluminum alloy. In hardness testing, the thick­ ness and the edge distance of the specimen being tested are two factors that must be con­ sidered to avoid distortion of the metal. Sev­ eral readings should be taken and the results averaged. In general, the higher the tensile strength, the greater its hardness. Common methods of hardness testing are outlined in the following paragraphs. These tests are suitable for determining the tensile properties resulting from the heat treatment of steel. Care should be taken to have case-hardened, corroded, pit­ ted, decarburized, or otherwise nonuniform surfaces removed to a sufficient depth. Exer­ cise caution not to cold-work, and conse­ quently harden, the steel during removal of the surface.

4-17. ROCKWELL HARDNESS TEST.

The Rockwell hardness test is the most com­ mon method for determining hardness of fer­ rous and many nonferrous metals. (See ta­ ble 4-5.) It differs from Brinell hardness test­ ing in that the hardness is determined by the depth of indentation made by a constant load impressing on an indenter. In this test, a stan­ dard minor load is applied to set a hardened steel ball or a diamond cone in the surface of the metal, followed by the application of a standard major load. The hardness is meas­ ured by depth of penetration. Rockwell super­ ficial hardness tests are made using light minor and major loads and a more sensitive system for measuring depth of indentation. It is useful for thin sections, very small parts, etc. Cali­ bration of Rockwell hardness testers is done in accordance with American Society of Testing Materials (ASTM E-18) specifications.

4-18. BRINELL HARDNESS TEST. In this test a standard constant load, usually 500 to 3,000 kg, is applied to a smooth flat metal surface by a hardened steel-ball type in­ denter, 10 mm in diameter. The 500-kg load is usually used for testing nonferrous metals such as copper and aluminum alloys, whereas the 3,000-kg load is most often used for testing harder metals such as steels and cast irons.

The numerical value of Brinell Hardness (HB), is equal to the load, divided by the surface area of the resulting spherical impression.

PHB = D(π [D − (D2 − d 2 ) ] ) 2 Where P is the load, in kg; D is the diameter of the ball, in mm; and d is the diameter of the indentation, in mm.

Par 4-16 Page 4-5

Page 146Open in PDF

a. General Precautions. To avoid mis­ application of Brinell hardness testing, the fundamentals and limitations of the test proce­ dure must be clearly understood. To avoid in­ accuracies, the following rules should be fol­ lowed.

(1) Do not make indentations on a curved surface having a radius of less than 1 inch.

(2) Do make the indentations with the correct spacing. Indentations should not be made too close to the edge of the work piece being tested.

(3) Apply the load steadily to avoid overloading caused by inertia of the weights.

(4) Apply the load so the direction of loading and the test surface are perpendicular to each other within 2 degrees.

(5) The thickness of the work piece being tested should be such that no bulge or mark showing the effect of the load appears on the side of the work piece opposite the inden­ tation.

(6) The indentation diameter should be clearly outlined.

b. Limitations. The Brinell hardness test has three principal limitations.

(1) The work piece must be capable of accommodating the relatively large indenta­ tions.

(2) Due to the relatively large indenta­ tions, the work piece should not be used after testing.

(3) The limit of hardness, 15 HB with the 500-kg load to 627 HB with the 3,000-kg load, is generally considered the practical range.

c. Calibration. A Brinell Hardness Tester should be calibrated to meet ASTM standard E10 specifications.

4-19. VICKERS HARDNESS TEST . In this test, a small pyramidal diamond is pressed into the metal being tested. The Vickers Hard­ ness number (HV) is the ratio of the load ap­ plied to the surface area of the indention. This is done with the following formula.

HV = P /.05 3 9 3 d 2

a. The indenter is made of diamond, and is in the form of a square-based pyramid hav­ ing an angle of 136 degrees between faces.

The facets are highly-polished, free from sur­ face imperfections, and the point is sharp. The loads applied vary from 1 to 120 kg; the stan­ dard loads are 5, 10, 20, 30, 50, 100, and 120 kg. For most hardness testing, 50 kg is maximum.

b. A Vickers hardness tester should be calibrated to meet ASTM standard E10 speci­ fications, acceptable for use over a loading range.

4-20. MICROHARDNESS TESTING .

This is an indentation hardness test made with loads not exceeding 1 kg (1,000 g). Such hardness tests have been made with a load as light as 1 g, although the majority of microhardness tests are made with loads of 100 to 500 g. In general, the term is related to the size of the indentation rather than to the load applied.

Page 4-6 Par 4-18

Page 147Open in PDF

a. Fields of Application . Microhardness testing is capable of providing information re­ garding the hardness characteristics of materi­ als which cannot be obtained by hardness tests such as the Brinell or Rockwell, and are as follows.

(1) Measuring the hardness of precision work pieces that are too small to be measured by the more common hardness-testing meth­ ods.

(2) Measuring the hardness of product forms such as foil or wire that are too thin or too small in diameter to be measured by the more conventional methods.

(3) Monitoring of carburizing or ni­ triding operations, which is sometimes accom­ plished by hardness surveys taken on cross sections of test pieces that accompanied the work pieces through production operations.

(4) Measuring the hardness of individ­ ual microconstituents.

(5) Measuring the hardness close to edges, thus detecting undesirable surface con­ ditions such as grinding burn and decarburiza­ tion.

(6) Measuring the hardness of surface layers such as plating or bonded layers.

b. Indenters. Microhardness testing can be performed with either the Knoop or the Vickers indenter. The Knoop indenter is used mostly in the United States; the Vickers in­ denter is the more widely used in Europe.

(1) Knoop indentation testing is per­ formed with a diamond, ground to pyramidal form, that produces a diamond-shaped inden­ tation with an approximate ratio between long and short diagonals of 7 to 1. The indentation depth is about one-thirtieth of its length. Due to the shape of the indenter, indentations of ac­ curately measurable length are obtained with light loads.

(2) The Knoop hardness number (HK) is the ratio of the load applied to the indenter to the unrecovered projected area of indenta­ tion. The formula for this follows.

H K=P/A =P/ Cl2 Where P is the applied load, in kg; A is the unrecovered projected area of indentation, in square mm; l is the measured length of the long diagonal, in mm; and C is 0.07028, a con­ stant of the indenter relating projected area of the indentation to the square of the length of the long diagonal.

4-21. INDENTATIONS. The Vickers in­ denter penetrates about twice as far into the work piece as does the Knoop indenter. The diagonal of the Vickers indentation is about one-third of the total length of the Knoop in­ dentation. The Vickers indenter is less sensi­ tive to minute differences in surface conditions than is the Knoop indenter. However, the Vickers indentation, because of the shorter di­ agonal, is more sensitive to errors in measuring than is the Knoop indentation. (See fig­ ure 4-1.)

FIGURE 4-1. Comparison of indentation made by Knoop and Vickers indenters in the same work metal and at the same loads.

Par 4-20 Page 4-7