Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 136–147
Page 148Open in PDF

4-22. MAGNETIC TESTING . Magnetic testing consists of determining whether the specimen is attracted by a magnet. Usually, a metal attracted by a magnet is iron, steel, or an iron-base alloy containing nickel, cobalt, or chromium. However, there are exceptions to this rule since some nickel and cobalt alloys may be either magnetic or nonmagnetic.

Never use this test as a final basis for identifi­ cation. The strongly attracted metals could be pure iron, pure nickel, cobalt, or iron-nickel­ cobalt alloys. The lightly attracted metals could be cold-worked stainless steel, or monel.

The nonmagnetic metals could be aluminum, magnesium, silver, or copper-base alloy, or an annealed 300-type stainless steel.

4-23. ALUMINUM TESTING . Hardness tests are useful for testing aluminum alloy chiefly as a means of distinguishing between annealed, cold-worked, heat-treated, and heattreated and aged material. It is of little value in indicating the strength or quality of heat treatment. Typical hardness values for alumi­ num alloys are shown in table 4-5.

a. Clad aluminum alloys have surface layers of pure aluminum or corrosion-resistant aluminum alloy bonded to the core material to inhibit corrosion. Presence of such a coating may be determined under a magnifying glass by examination of the edge surface which will show three distinct layers. In aluminum alloys, the properties of any specific alloy can be al­ tered by work hardening (often called strainhardening), heat treatment, or by a combina­ tion of these processes.

b. Test for distinguishing heat-treatable and nonheat-treatable aluminum alloys . If for any reason the identification mark of the alloy is not on the material, it is possible to distinguish between some heat-treatable alloys and some nonheat-treatable alloys by immers­ ing a sample of the material in a 10 percent solution of caustic soda (sodium hydroxide).

Those heat-treated alloys containing several percent of copper (2014, 2017, and 2024) will turn black due to the copper content. Highcopper alloys when clad will not turn black on the surface, but the edges will turn black at the center of the sheet where the core is exposed.

If the alloy does not turn black in the caustic soda solution it is not evidence that the alloy is nonheat-treatable, as various high-strength heat-treatable alloys are not based primarily on the use of copper as an alloying agent. These include among others 6053, 6061, and 7075 alloys. The composition and heattreating ability of alloys which do not turn black in a caustic soda solution can be estab­ lished only by chemical or spectro-analysis.

TABLE 4-5. Hardness values for aluminum alloys. (Ref­ erence MIL-H-6088G .)

Hardness Brinell number Commercial Temper 500 kg. load Designation 10 mm. ball Material 1100 0 23 H18 44 3003 0 28 H16 47 2014 0 45 T6 135 2017 0 45 T6 105 2024 0 47 T4 120 2025 T6 110 6151 T6 100 5052 0 47 H36 73 6061 0 30 T4 65 T6 95 7075 T6 135 7079 T6 135 195 T6 75 220 T4 75 C355 T6 80 A356 T6 70

4-24.  4-35. [RESERVED.]

Page 4-8 Par 4-22

Page 149Open in PDF

SECTION 3. PRECAUTIONARY MEASURES

4-36. FLUTTER AND VIBRATION PRECAUTIONS. To prevent the occurrence of severe vibration or flutter of flight control surfaces during flight, precautions must be taken to stay within the design balance limita­ tions when performing maintenance or repair.

a. Balance Changes. The importance of retaining the proper balance and rigidity of air­ craft control surfaces cannot be overempha­ sized. The effect of repair or weight change on the balance and center of gravity is proportion­ ately greater on lighter surfaces than on the older heavier designs. As a general rule, repair the control surface in such a manner that the weight distribution is not affected in any way, in order to preclude the occurrence of flutter of the control surface in flight. Under certain conditions, counter-balance weight is added forward of the hinge line to maintain balance.

Add or remove balance weights only when necessary in accordance with the manufac­ turer’s instructions. Flight testing must be ac­ complished to ensure flutter is not a problem.

Failure to check and retain control surface bal­ ance within the original or maximum allow­ able value could result in a serious flight hazard.

b. Painting and Refinishing. Special emphasis is directed to the effect of too many extra coats of paint on balanced control sur­ faces. Mechanics must avoid adding addi­ tional coats of paint in excess of what the manufacturer originally applied. If available consult the aircraft manufacturer’s instructions relative to finishing and balance of control surfaces.

c. Trapped Water or Ice. Instances of flutter have occurred from unbalanced condi­ tions caused by the collection of water or ice within the surface. Therefore, ventilation and drainage provisions must be checked and re­ tained when maintenance is being done.

d. Trim Tab Maintenance. Loose or vi­ brating trim tabs will increase wear of actuat­ ing mechanisms and hinge points which may develop into serious flutter conditions. When this happens, primary control surfaces are highly susceptible to wear, deformation, and fatigue failures because of the buffeting nature of the airflow over the tab mechanism. Trail­ ing-edge play of the tab may increase, creating an unsafe flutter condition. Careful inspection of the tab and its mechanism should be con­ ducted during overhaul and annual inspection periods. Compared to other flight control sys­ tems on the aircraft, only a minor amount of tab-mechanism wear can be tolerated.

(1) Free play and stiffness may best be measured by a simple static test where “up­ ward” and “downward” (or “leftward” and “rightward”) point forces are applied near the trailing edge of the tab at the span-wise at­ tachment of the actuator (so as not to twist the tab). The control surface to which the trim tab is attached should be locked in place. Rota­ tional deflection readings are then taken near the tab trailing edge using an appropriate measuring device, such as a dial gauge. Sev­ eral deflection readings should be taken using loads first applied in one direction, then in the opposite. If the tab span does not exceed 35 percent of the span of the supporting con­ trol surface, the total free play at the tab trail­ ing edge should not exceed 2 percent of the tab chord. If the tab span equals or exceeds 35 percent of the span of the supporting con­ trol surface, the total free play at the tab trail­ ing edge should not exceed 1 percent of the distance from the tab hinge line to the trailing edge of the tab perpendicular to the tab hinge line. For example, a tab that has a chord of Par 4-36 Page 4-9

Page 150Open in PDF

4 inches and less than or equal to 35 percent of the control surface span would have a maxi­ mum permissible free play of 4 inches x 0.020 or 0.080 inches (total motion up and down) measured at the trailing edge. Correct any free play in excess of this amount.

(2) Care must also be exercised during repair or rework to prevent stress concentration points or areas that could increase the fatigue susceptibility of the trim tab system. Advisory Circular (AC) 23.629-1A, Means of Compli­ ance with Section 23.629, “Flutter,” contains additional information on this subject.

NOTE: If the pilot has experienced flutter, or thinks he/she has, then a complete inspection of the aircraft flight control system and all related components including rod ends, bearings, hinges, and bellcranks must be accomplished. Suspected parts should be replaced.

4-37. LOAD FACTORS FOR REPAIRS.

In order to design an effective repair to a sheet metal aircraft, the stresses that act on the structure must be understood.

a. Six types of major stresses are known and should be considered when making re­ pairs. These are tension, compression, bend­ ing, torsion, shear, and bearing

b. The design of an aircraft repair is complicated by the requirement that it be as light as possible. If weight were not critical, repairs could be made with a large margin of safety. But in actual practice, repairs must be strong enough to carry all of the loads with the required factor of safety, but they must not have too much extra strength. A joint that is too weak cannot be tolerated, but neither can one that is too strong because it can create stress risers that may cause cracks in other lo­ cations.

4-38. TRANSFER OF STRESSES WITH - IN A STRUCTURE. An aircraft structure must be designed in such a way that it will ac­ cept all of the stresses imposed upon it by the flight and ground loads without any permanent deformation. Any repair made must accept the stresses, carry them across the repair, and then transfer them back into the original structure.

These stresses are considered as flowing through the structure, so there must be a con­ tinuous path for them, with no abrupt changes in cross-sectional areas along the way. Abrupt changes in cross-sectional areas of aircraft structure that are subject to cycle load­ ing/stresses will result in stress concentration that may induce fatigue cracking and eventual failure. A scratch or gouge in the surface of a highly-stressed piece of metal will cause a stress concentration at the point of damage.

a. Multirow Fastener Load Transfer.

When multiple rows of rivets are used to se­ cure a lap joint, the transfer of stresses is not equal in each row. The transfer of stress at each row of rivets may be thought of as trans­ ferring the maximum amount capable of being transferred without experiencing rivet shear failure.

b. Use Of Stacked Doublers. A stacked doubler is composed of two or more sheets of material that are used in lieu of a single, thicker sheet of material. Because the stress transferred at each row of rivets is dependent upon the maximum stress that can be trans­ ferred by the rivets in that row, the thickness of the sheet material at that row need only be thick enough to transfer the stress applied.

Employing this principle can reduce the weight of a repair joint.

4-39.  4-49. [RESERVED.] Page 4-10 Par 4-36

Page 151Open in PDF

SECTION 4. METAL REPAIR PROCEDURES

4-50. GENERAL. The airframe of a fixedwing aircraft is generally considered to consist of five principal units; the fuselage, wings, stabilizers, flight control surfaces, and landing gear.

a. Aircraft principal structural elements (PSE) and joints are designed to carry loads by distributing them as stresses. The elements and joints as originally fabricated are strong enough to resist these stresses, and must re­ main so after any repairs. Long, thin elements are called members. Some examples of mem­ bers are the metal tubes that form engine mount and fuselage trusses and frames, beams used as wing spars, and longerons and string­ ers of metal-skinned fuselages and wings.

Longerons and stringers are designed to carry principally axial loads, but are sometimes re­ quired to carry side loads and bending mo­ ments, as when they frame cutouts in metal-skinned structures. Truss members are designed to carry axial (tension and compres­ sion) loads applied to their ends only. Frame members are designed to carry side loads and bending moments in addition to axial loads.

Beam members are designed to carry side loads and bending moments that are usually large compared to their axial loads. Beams that must resist large axial loads, particularly compression loads, in combination with side loads and bending moments are called beam-columns. Other structural elements such as metal skins, plates, shells, wing ribs, bulk­ heads, ring frames, intercostal members, gus­ sets, and other reinforcements, and fittings are designed to resist complex stresses, sometimes in three dimensions.

b. Any repair made on an aircraft struc­ ture must allow all of the stresses to enter, sustain these stresses, and then allow them to return into the structure. The repair must be equal to the original structure, but not stronger or stiffer, which will cause stress concentra­ tions or alter the resonant frequency of the structure.

c. All-metal aircraft are made of very thin sheet metal, and it is possible to restore the strength of the skin without restoring its ri­ gidity. All repairs should be made using the same type and thickness of material that was used in the original structure. If the original skin had corrugations or flanges for rigidity, these must be preserved and strengthened. If a flange or corrugation is dented or cracked, the material loses much of its rigidity; and it must be repaired in such a way that will restore its rigidity, stiffness, and strength.

4-51. RIVETED (OR BOLTED) STEEL TRUSS-TYPE STRUCTURES. Repairs to riveted structures may be made employing the general principles outlined in the following paragraphs on aluminum alloy structures. Re­ pair methods may also be found in text books on metal structures. Methods for repair of the major structural members must be specifically approved by the Federal Aviation Administra­ tion (FAA).

4-52. ALUMINUM ALLOY STRUC­ TURES. Extensive repairs to damaged stressed skin on monocoque-types of alumi­ num alloy structures must be made in accor­ dance with FAA-approved manufacturer’s in­ structions or other FAA-approved source.

a. Rivet Holes. Rivet holes are slightly larger than the diameter of the rivet. When driven, solid rivets expand to fill the hole. The strength of a riveted joint is based upon the expanded diameter of the rivet. Therefore, it is important that the proper drill size be used for each rivet diameter.

Par 4-50 Page 4-11

Page 152Open in PDF

(1) The acceptable drill size for rivets may be found in Metallic Materials and Ele­ ments for Flight Vehicle Structure (MIL-HDBK-5).

(2) Avoid drilling oversized holes or otherwise decreasing the effective tensile areas of wing-spar capstrips, wing, fuselage, finlongitudinal stringers, or highly-stressed ten­ sile members. Make all repairs, or reinforce­ ments, to such members in accordance with factory recommendations or with the specific approval of an FAA representative.

b. Disassembly Prior to Repairing. I f the parts to be removed are essential to the ri­ gidity of the complete structure, support the structure prior to disassembly in such a manner as to prevent distortion and permanent damage to the remainder of the structure. When rivets are removed, undercut rivet heads by drilling.

Use a drill of the same size as the diameter of the rivet. Drilling must be exactly centered and to the base of the head only. After drill­ ing, break off the head with a pin punch and carefully drive out the shank. On thin or un­ supported metal skin, support the sheet metal on the inside with a bucking bar. Removal of rivet heads with a cold chisel and hammer is not recommended because skin damage and distorted rivet holes will probably result. In­ spect rivet joints adjacent to damaged structure for partial failure by removing one or more rivets to see if holes are elongated or the rivets have started to shear.

c. Effective Tools. Care must also be taken whenever screws must be removed to avoid damage to adjoining structure. When properly used, impact wrenches can be effec­ tive tools for removal of screws; however, damage to adjoining structure may result from excessive vertical loads applied through the screw axis. Excessive loads are usually related to improperly adjusted impact tools or at­ tempting to remove screws that have seized from corrosion. Remove seized screws by drilling and use of a screw extractor. Once the screw has been removed, check for structural cracks that may appear in the adjoining skin doubler, or in the nut or anchor plate.

4-53. SELECTION OF ALUMINUM FOR REPLACEMENT PARTS. All alumi­ num replacement sheet metal must be identical to the original or properly altered skin. If an­ other alloy is being considered, refer to the in­ formation on the comparative strength proper­ ties of aluminum alloys contained in MIL-HDBK-5.

a. Temper. The choice of temper depends upon the severity of the subsequent forming operations. Parts having single curvature and straight bend lines with a large bend radius may be advantageously formed from heat-treated material; while a part, such as a fuselage frame, would have to be formed from a soft, annealed sheet, and heat-treated after forming. Make sure sheet metal parts which are to be left unpainted are made of clad (alu­ minum coated) material. Make sure all sheet material and finished parts are free from cracks, scratches, kinks, tool marks, corrosion pits, and other defects which may be factors in subsequent failure.

b. Use of Annealed Alloys for Struc­ tural Parts. The use of annealed aluminum alloys for structural repair of an aircraft is not recommended. An equivalent strength repair using annealed aluminum will weigh more than a repair using heat-treated aluminum alloy.

4-54. HEAT TREATMENT OF ALUMI­ NUM ALLOY PARTS. All structural alumi­ num alloy parts are to be heat-treated in accor­ dance with the heat-treatment instruction is­ sued by the manufacturers of the part. In the case of a specified temper, the sequence of heat-treating operations set forth in Page 4-12 Par 4-52

Page 153Open in PDF

MIL-HDBK-5 and corresponding specifica­ tions. If the heat-treatment produces warping, straighten the parts immediately after quench­ ing. Heat-treat riveted parts before riveting, to preclude warping and corrosion.

a. Quenching. Quench material from the solution heat-treating temperature as rapidly as possible after removal from the furnace.

Quenching in cold water is preferred, although less drastic chilling (hot or boiling water, or airblast) is sometimes employed for bulk sec­ tions, such as forgings, to minimize quenching stresses.

b. Reheating at Temperatures Above Boiling Water. Reheating of 2017 and 2024 alloys above 212 °F tend to impair the original heat treatment. Therefore, reheating above 212 °F, including the baking of primers, is not acceptable without subsequent complete and correct heat treatment.

4-55. BENDING METAL. When describ­ ing a bend in aviation, the term “bend radii” is used to refer to the inside radius. Require­ ments for bending the metal to various shapes are frequently encountered. When a metal is bent, it is subjected to changes in its grain structure, causing an increase in its hardness.

a. The minimum radius is determined by the composition of the metal, its temper, and thickness. Table 4-6 shows the recommended radius for different types of aluminum. Note that the smaller the thickness of the material, the smaller the recommended minimum bend radius, and that as the material increases in hardness, the recommended bend radii in­ creases.

b. When using layout techniques, the mechanic must be able to calculate exactly how much material will be required for the bend. It is easier to lay out the part on a flat sheet before the bending or shaping is per­ formed. Before bending, smooth all rough edges, remove burrs, and drill relief holes at the ends of bend lines and at corners; to pre­ vent cracks from starting. Bend lines should preferably be made to lie at an angle to the grain of the metal (preferably 90 degrees).

c. Bend radii (BR) in inches for a spe­ cific metal composition (alloy) and temper is determined from table 4-6. For example, the minimum bend radii for 0.016 thick 2024-T6 (alloy and temper) is found is found to be 2 to 4 times the material thickness or

0.032 to 0.064.

4-56. SETBACK.

a. Setback is a measurement used in sheet metal layout. It is the distance the jaws of a brake must be setback from the mold line to form a bend. For a 90 degree bend, the point is back from the mold line to a distance equal to the bend radius plus the metal thickness.

The mold line is an extension of the flat side of a part beyond the radius. The mold line di­ mension of a part, is the dimension made to the intersection of mold lines, and is the di­ mension the part would have if its corners had no radius. (See figure 4-2.)

FIGURE 4-2. Setback for a 90-degree bend.

Par 4-54 Page 4-13

Page 154Open in PDF

TABLE 4-6. Recommended radii for 90-degree bends in aluminum alloys.

Alloy and Approximate sheet thickness (t) (inch) temper 0.016 0.032 0.064 0.128 0.182 0.258 2024-01 0 0-1t 0-1t 0-1t 0-1t0-1t 0-1t 2024-T31, 2 1½t-3t 2t-4t 3t-5t 4t-6t 4t-6t 5t-7t 2024-T61 2t-4t 3t-5t 3t-5t 4t-6t 5t-7t 6t-10t 5052-0 0 0 0-1t 0-1t 0-1t 0-1t 5052-H32 0 0 ½t-1t ½t-1½t ½t-1½t ½t-1½t 5052-H34 0 0 ½t-1½t 1½t-2½t 1½t-2½t 2t-3t 5052-H36 0-1t ½t-1½t 1t-2t 1½t-3t 2t-4t 2t-4t 5052-H38 ½t-1½t 1t-2t 1½t-3t 2t-4t 3t-5t 4t-6t 6061-0 0 0-1t 0-1t 0-1t 0-1t 0-1t 6061-T4 0-1t 0-1t ½t-1½t 1t-2t 1½t-3t 2½t-4t 6061-T6 0-1t ½t-1½t 1t-2t 1½t-3t 2t-4t 3t-4t 7075-0 0 0-1t 0-1t ½t-1½t 1t-2t 1½t-3t 7075-T61 2t-4t 3t-5t 4t-6t 5t-7t 5t-7t 6t-10t 1 Alclad sheet may be bent over slightly smaller radii than the corresponding tempers of uncoated alloy.

2 Immediately after quenching, this alloy may be formed over appreciably smaller radii.

b. To determine setback for a bend of more or less than 90 degrees, a correction known as a K-factor must be applied to find the setback.

(1) Table 4-7 shows a chart of K-factors. To find the setback for any degree of bend, multiply the sum of the bend radius and metal thickness by the K-value for the an­ gle through which the metal is bent.

(2) Figure 4-3 shows an example of a piece of 0.064 inch sheet metal bent through 45 degrees to form an open angle of 135 degrees. For 45 degrees, the K-factor is 0.41421. The setback, or the distance from the mold point to the bend tangent line, is:

Setback = K(BR + MT) = 0.41421 (0.25 + 0.064) = 0.130 inches

(3) If a closed angle of 45 degrees is formed, the metal must be bent through 135 degrees. The K-factor for 135 de­ grees is 2.4142, so the setback, or distance from the mold point to the bend tangent line, is

0.758 inch.

4-57. RIVETING .

a. The two major types of rivets used in aircraft are the common solid shank rivet, which must be driven using an air-driven rivet gun and bucking bar; and special (blind) rivets, which are installed with special installation tools. Design allowables for riveted assem­ blies are specified in MIL-HDBK-5.

(1) Solid shank rivets are used widely during assembly and repair work. They are identified by the material of which they are made, the head type, size of shank, and temper condition.

Page 4-14 Par 4-56

Page 155Open in PDF

TABLE 4-7. K-chart for determining setback for bends other than 90 degrees.

Deg. K D e g . K D eg. K D e g . K D e g : K 1 0.0087 37 0.3346 73 0.7399 109 1.401 145 3.171 2 3

0.0174

0.0261 38 39

0.3443

0.3541 74 0.7535 75 0.7673 110 1,428 111 1.455 146 3.270 147 3.375 4 0.0349 40 0.3639 76 0.7812 112 1.482 148 3.487 5 0.0436 41 0.3738 77 0.7954 113 1.510 149 3.605 6 0.0524 42 0.3838 78 0.8097 114 1.539 150 3.732 7 0.0611 43 0.3939 79 0.8243 115 1.569 151 3.866 8 0.0699 44 0.4040 80 0.8391 116 1.600 152 4.010 9 0.0787 45 0.4142 81 0.8540 117 1.631 153 4.165 10 0.0874 46 0.4244 82 0.8692 118 1.664 154 4.331 11 0.0963 47 0.4348 83 0.8847 119 1.697 155 4.510 12 0.1051 48 0.4452 84 0.9004 120 1.732 156 4.704 13 0.1139 49 0.4557 85 0.9163 121 1.767 157 4.915 14 0.1228 50 0.4663 86 0.9324 122 1.804 158 5.144 15 0.1316 51 0.4769 87 0.9489 123 1.841 159 5.399 16 0.1405 52 0.4877 88 0.9656 124 1.880 160 5.671 17 0.1494 53 0.4985 89 0.9827 125 1.921 161 5.975 18 0.1583 54 0.5095 90 1.000 126 1.962 162 6.313 19 0.1673 55 0.5205 91 1.017 127 2.005 163 6.691 20 0.1763 56 0.5317 92 1.035 128 2.050 164 7.115 21 0.1853 57 0.5429 93 1.053 129 2.096 165 7.595 22 0.1943 58 0.5543 94 1.072 130 2.144 166 8.144 23 0.2034 59 0.5657 95 1.091 131 2.194 167 8.776 24 0.2125 60 0.5773 96 1.110 132 2.246 168 9.514 25 0.2216 61 0.5890 97 1-130 133 2.299 169 10.38 26 0.2308 62 0.6008 98 1.150 134 2.355 170 11.43 27 0.2400 63 0.6128 99 1.170 135 2.414 171 12.70 28 0.2493 64 0.6248 100 1.191 136 2.475 172 14.30 29 0.2586 65 0.6370 101 1.213 137 2.538 173 16.35 30 0.2679 66 0.6494 102 1.234 138 2.605 174 19.08 31 0.2773 67 0.6618 103 1.257 139 2.674 175 22.90 32 0.2867 68 0.6745 104 1.279 140 2.747 176 26.63 33 0.2962 69 0.6872 105 1.303 141 2.823 177 38.18 34 0.3057 70 0.7002 106 1.327 142 2.904 178 57.29 35 0.3153 71 0.7132 107 1.351 143 2.988 179 114.59 36 0.3249 72 0.7265 108 1.376 144 3.077 180 Inf.

(2) The material used for the majority of solid shank rivets is aluminum alloy. The strength and temper conditions of aluminum alloy rivets are identified by digits and letters similar to those used to identify sheet stock.

The 1100, 2017-T, 2024-T, 2117-T, and 5056 rivets are the six grades usually available.

AN-type aircraft solid rivets can be identified by code markings on the rivet heads. A rivet made of 1100 material is designated as an “A” rivet, and has no head marking. The 2017-T alloy rivet is designated as a “D” rivet and has a raised teat on the head. Two dashes on a rivet head indicate a 2024-T alloy desig­ nated as a “DD” rivet. The 2117-T rivet is designated as an “AD” rivet, and has a dimple on the head. A “B” designation is given to a rivet of 5056 material and is marked with a raised cross on the rivet head. Each type of rivet is identified by a part number to allow the user to select the correct rivet. The numbers are in series and each series represents a par­ ticular type of head. (See figure 4-4 and ta­ ble 4-8.)

(3) An example of identification mark­ ing of rivet follows.

MS 20470AD3-5 Complete part number MS Military standard number 20470 Universal head rivet AD 2117-T aluminum alloy 3 3/32nds in diameter 5 5/16ths in length Par 4-57 Page 4-15

Page 156OCROpen in PDF

RIVET IDENTIFICATION T = 0.064" The material can be identified by the head marking Material R = 0.250 Rivet Code Head Marking Material SETBACK O¢ A PLAIN (Dyed) 1100 AD DIMPLED 2117

•- SETBACK D RAISED DOT 2017T This is a 90-degree angle.

Setback = BR + MT DO TWO RAISED DASHES 2024 = 0.250 + 0.064 = 0.314" RAISED CROSS (Dyed) 5056 T = 0.064" RAISED CIRCLE 7050 M TWO DOTS Monel R = 0.250

PART NUMBER BREAKDOWN

•MS20470 AD 4-7

SETBACK This is a 135-degree open angle. The metal has only been bent 45°.

SB = (BR + MT)K MS20470 • •• AD • = (0.250 + 0.064) 0.4121 = 0.130" Type Head Material Diameter Length Code Measured Measured T = 0.064 in 32nds in 16ths of an inch of an inch Length is measured from the SETBACK ength top of the flush head and the

• R = 0.250 underside of the universal head

SETBACK This is a 45 degree closed angle.

Setback = (BR + MT)K = (0.250 + 0.064)2.4142 = 0.758" FIGURE 4-3. Methods of determining setback for bends other than 90 degree.

(4) Countersunk head rivets (MS20426 supersedes AN426 100-degree) are used where a smooth finish is desired. The 100-degree countersunk head has been adopted as the standard in the United States. The universal head rivet (AN470 superseded by MS20470) has been adopted as the standard for protruding-head rivets, and may be used as a replacement for the roundhead, flathead, and brazier head rivet. These rivets can also be purchased in half sizes by designating a "0.5" after the main length (i.e., MS20470 AD4-3.5).

FIGURE 4-4. Rivet identification and part number breakdown.

b. Replace rivets with those of the same size and strength whenever possible. If the rivet hole becomes enlarged, deformed, or otherwise damaged; drill or ream the hole for the next larger size rivet. However, make sure that the edge distance and spacing is not less than minimums listed in the next paragraph. Rivets may not be replaced by a type having lower strength properties, unless the lower strength is adequately compensated by an increase in size or a greater number of rivets. It is acceptable to replace 2017 rivets of 3/16 inch diameter or less, and 2024 rivets of 5/32 inch diameter or less with 2117 rivets for general repairs, provided the replacement rivets are 1/32 inch greater in diameter than the rivets they replace.

Page 4-16 Par 4-57

Page 157Open in PDF

TABLE 4-8. Aircraft rivet identification.

Material 1100 2117T 2017T 2017T-HD 2024T 5056T 7075-T73 Head Marking Plain Dimpled Raised Dot Raised Dot Raised Double Dash Raised Cross Three Raised Dashes AN Material Code

A AD D D DD B AN425 78�� �� Counter- Sunk Head

X X X X X X AN426 100�� �� Counter- Sunk Head MS20426

X X X X X X X AN427 100�� �� Counter- Sunk Head MS20427 AN430 Round Head MS20470

X X X X X X X AN435 Round Head MS20613 MS20615 AN 441 Flat Head AN 442 Flat Head MS20470

X X X X X X X AN 455 Brazier Head MS20470

X X X X X X X AN 456 Brazier Head MS20470

X X X X X X X AN 470 Universal Head MS20470

X X X X X X X Heat Treat Before Using No No Yes No Yes No No Shear Strength psi 10000 30000 34000 38000 41000 27000 Bearing Strength psi 25000 100000 113000 126000 136000 90000 Par 4-57 Page 4-17

Page 158Open in PDF

TABLE 4-8. Aircraft rivet identification. (continued) Material Carbon Steel Corrosion- Resistant Steel Copper Monel Monel Nickel- Copper Alloy Brass Titanium Head Marking Recessed Triangle Recessed Dash Plain Plain Recessed Double Dots Plain Recessed Large and Small Dot AN Material Code

F C M C AN425 78�� �� Counter- Sunk Head AN426 100�� �� Counter- Sunk Head MS20426 MS 20426 AN427 100�� �� Counter- Sunk Head MS20427

X X X X AN430 Round Head MS20470 AN435 Round Head MS20613 MS20615 X MS20613 X MS20613 X X MS20615 X MS20615 AN 441 Flat Head

X X X X AN 442 Flat Head MS20470 AN 455 Brazier Head MS20470 AN 456 Brazier Head MS20470 AN 470 Universal Head MS20470 Heat Treat Before Using No No No No No No No Shear Strength psi 35000 65000 23000 49000 49000 95000 Bearing Strength psi 90000 90000 Page 4-18 Par 4-57

Page 159Open in PDF

c. Rivet edge distance is defined as the distance from the center of the rivet hole to the nearest edge of the sheet. Rivet spacing is the distance from the center of the rivet hole to the center of the adjacent rivet hole. Unless structural deficiencies are suspected, the rivet spacing and edge distance should duplicate those of the original aircraft structure. If structural deficiencies are suspected, the fol­ lowing may be used in determining minimum edge distance and rivet spacing.

(1) For single row rivets, the edge dis­ tance should not be less than 2 times the di­ ameter of the rivet and spacing should not be less than 3 times the diameter of the rivet.

(2) For double row rivets, the edge dis­ tance and spacing should not be less than the minimums shown in figure 4-5.

(3) For triple or multiple row rivets, the edge distance and spacing should not be less than the minimums shown in figure 4-5.

d. The 2117 rivets may be driven in the condition received, but 2017 rivets above 3/16 inch in diameter and all 2024 rivets are to be kept packed in dry ice or refrigerated in the “quenched” condition until driven, or be reheat treated just prior to driving, as they would oth­ erwise be too hard for satisfactory riveting.

Dimensions for formed rivet heads are shown in figure 4-6(a), together with commonly found rivet imperfections.

e. When solid shank rivets are impracti­ cal to use, then special fasteners are used.

Special fastening systems used for aircraft construction and repair are divided into two types, special and blind fasteners. Special fasteners are sometimes designed for a specific purpose in an aircraft structure. The name “special fasteners” refers to its job requirement and the tooling needed for installation. Use of special fasteners may require an FAA field ap­ proval.

f. Blind rivets are used under certain con­ ditions when there is access to only one side of the structure. Typically, the locking charac­ teristics of a blind rivet are not as good as a driven rivet. Therefore, blind rivets are usually not used when driven rivets can be installed.

Blind rivets shall not be used:

(1) in fluid-tight areas;

(2) on aircraft in air intake areas where rivet parts may be ingested by the engine, on aircraft control surfaces, hinges, hinge brack­ ets, flight control actuating systems, wing at­ tachment fittings, landing gear fittings, on floats or amphibian hulls below the water level, or other heavily-stressed locations on the aircraft;

CAUTION: For metal repairs to the air­ frame, the use of blind rivets must be spe­ cifically authorized by the airframe manu­ facturer or approved by a representative of the FAA.

(3) Self plugging friction-lock cherry rivets. This patented rivet may be installed when there is access to only one side of the structure. The blind head is formed by pulling the tapered stem into the hollow shank. This swells the shank and clamps the skins tightly together. When the shank is fully upset, the stem pulls in two. The stem does not fracture flush with the rivet head and must be trimmed and filed flush for the installation to be com­ plete. Because of the friction-locking stem, these rivets are very sensitive to vibrations.

Inspection is visual, with a loose rivet standing out in the standard “smoking rivet” pattern.

Removal consists of punching out the friction- Par 4-57 Page 4-19 (and 4-19a)