AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 186–197
Page 198Open in PDF

(2) The 250+ amp arc between the electrode and the work melts the metal at 5,432 ºF, and a filler rod is manually fed into the molten puddle. A stream of inert gas such as argon or helium flows out of the torch and envelopes the arc, thereby preventing the formation of oxides in the puddle.

(3) The versatility of TIG welding is in­ creased by the power supply that is used. Di­ rect current of either polarity or alternating current may be used. (See figures 4-29 and 4-30.)

FIGURE 4-29. Set TIG welder to DC current, straight polarity for welding mild steel, stainless steel and ti­ tanium FIGURE 4-30. Set TIG to AC current for welding aluminum and magnesium.

4-87. ELECTRIC-RESISTANCE WELD­ ING. Many thin sheet metal parts for aircraft, especially stainless steel parts, are joined by one of the forms of electric resistance welding, either spot welding or seam welding.

a. Spot Welding. Two copper electrodes are held in the jaws of the spot welding machine, and the material to be welded is clamped be­ tween them. Pressure is applied to hold the electrodes tightly together, and electrical cur­ rent flows through the electrodes and the mate­ rial. The resistance of the material being welded is so much higher than that of the cop­ per electrodes that enough heat is generated to melt the metal. The pressure on the electrodes forces the molten spots in the two pieces of metal to unite, and this pressure is held after the current stops flowing long enough for the metal to solidify. Refer to MIL HDBK-5 for joint construction and strength data. The amount of current, pressure, and dwell time are all carefully controlled and matched to the type of material and the thickness to produce the cor­ rect spot welds. (See figure 4-31.)

b. Seam Welding. Rather than having to release the electrodes and move the material to form a series of overlapping spot welds, a seam-welding machine is used to manufacture FIGURE 4-31. In spot welding, heat is produced by electrical resistance between copper electrodes. Pres­ sure is simultaneously applied to electrode tips to force metal together to complete fusing process. Spot-weld­ nugget size is directly related to tip size.

fuel tanks and other components where a con­ tinuous weld is needed. Two copper wheels Page 4-58 Par 4-86

Page 199Open in PDF

replace the bar-shaped electrodes. The metal to be welded is moved between them, and electric pulses create spots of molten metal that overlap to form the continuous seam.

4-88. BRAZING. Brazing refers to a group of metal-joining processes in which the bond­ ing material is a nonferrous metal or alloy with a melting point higher than 425 C (800 F), but lower than that of the metals being joined.

Brazing includes silver brazing (erroneously called silver soldering or hard soldering), cop­ per brazing, and aluminum brazing.

NOTE: Never weld over a previously brazed joint.

a. Brazing requires less heat than welding and can be used to join metals that are dam­ aged by high heat. However, because the strength of brazed joints is not as great as welded joints, brazing is not used for structural repairs on aircraft. In deciding whether braz­ ing of a joint is justified, it should be remem­ bered that a metal, which will be subjected to a sustained high temperature in use, should not be brazed.

b. A brazing flux is necessary to obtain a good union between the clean base metal and the filler metal. There are a number of readily available manufactured fluxes conforming to AWS and AMT specifications.

c. The base metal should be preheated slowly with a mild flame. When it reaches a dull-red heat (in the case of steel), the rod should be heated to a dark (or purple) color and dipped into the flux. Since enough flux adheres to the rod, it is not necessary to spread it over the surface of the metal.

d. A neutral flame is used in most brazing applications. However, a slightly oxidizing flame should be used when copper-zinc, copper-zinc-silicon, or copper-zinc-nickel-silicon filler alloys are used. When brazing aluminum and its alloys, a neutral flame is preferred, but if difficulties are encountered, a slightly re­ duced flame is preferred to an oxidizing flame.

e. The filler rod can now be brought near the tip of the torch, causing the molten bronze to flow over a small area of the seam. The base metal must be at the flowing temperature of the filler metal before it will flow into the joint. The brazing metal melts when applied to the steel and runs into the joint by capillary at­ traction. In braze welding, the rod should continue to be added, as the brazing pro­ gresses, with a rhythmic dipping action; so that the bead will be built to a uniform width and height. The job should be completed rapidly and with as few passes of the rod and torch as possible.

f. When the job is finished, the metal should be allowed to cool slowly. After cool­ ing, remove the flux from the parts by im­ mersing them for 30 minutes in a lye solution.

(1) Copper brazing of steel is normally done in a special furnace having a controlled atmos­ phere, and at a temperature so high that field repairs are seldom feasible. If copper brazing is attempted without a controlled atmosphere, the copper will probably not completely wet and fill the joint. Therefore, c opper brazing in any conditions other than appropriately con­ trolled conditions is not recommended.

(a) The allowable shear strength for copper brazing of steel alloys should be 15 thousand pounds per square inch (kpsi), for all condi­ tions of heat treatment.

(b) The effect of the brazing process on the strength of the parent or base metal of steel alloys should be considered in the structural design. Where copper furnace brazing is em­ ployed, the calculated allowable strength of Par 4-87 Page 4-59

Page 200Open in PDF

the base metal, which is subjected to the tem­ peratures of the brazing process, should be in accordance with table 4-14.

TABLE 4-14. Calculated allowable strength of base metal.

Material Allowable Strength Heat-treated material (in­ cluding normalized) used in “as-brazed” condition Mechanical properties of normalized material Heat-treated material (in­ cluding normalized) reheat-treated during or after brazing Mechanical properties corresponding to heat treatment performed

(2) Alloys commonly referred to as silver solders melt above 425 °C (800 °F), and when using them the process should be called silver brazing.

(a) The principal use of silver brazing in air­ craft work is in the fabrication of high-pressure oxygen lines and other parts which must with­ stand vibration and high temperatures. Silver brazing is used extensively to join copper (and its alloys), nickel, silver, various combinations of these metals, and thin steel parts. Silver brazing produces joints of higher strength than those produced by other brazing processes.

(b) It is necessary to use flux in all silverbrazing operations, because of the necessity for having the base metal chemically clean, (with­ out the slightest film of oxide to prevent the silver-brazing alloy from coming into intimate contact with the base metal).

(c) The joint must be physically and chemi­ cally clean, which means it must be free of all dirt, grease, oil, and paint. After removing the dirt, grease, and paint, any oxide should be removed by grinding or filing the piece until bright metal can be seen. During the soldering operation, the flux continues the process of keeping oxide away from the metal and aids the flow of solder.

(d) In figure 4-32, three types of joints for silver brazing are shown; flanged butt, lap, and edge joints. If a lap joint is used, the amount of lap should be determined according to the strength needed in the joint. For strength equal to that of the base metal in the heated zone, the amount of lap should be four to six times the metal thickness.

FIGURE 4-32. Silver brazing joints.

(e) The oxyacetylene flame for silver brazing should be neutral, but may have a slight excess of acetylene. It must be soft, not harsh. Dur­ ing both preheating and application of the sol­ der, the tip of the inner cone of the flame should be held about 1/2 inch from the work.

The flame should be kept moving so that the metal will not become overheated.

(f) When both parts of the base metal are at the right temperature (indicated by the flow of flux), brazing alloy can be applied to the sur­ face of the under or inner part at the edge of the seam. It is necessary to simultaneously di­ rect the flame over the seam, and keep moving it so that the base metal remains at an even temperature.

Page 4-60 Par 4-88

Page 201Open in PDF

(3) The torch can be shut off simply by closing the acetylene off first and allowing the gas remaining in the torch tip to burn out.

Then turn off the oxygen valve. If the torch is not to be used again for a long period, the pressure should be turned off at the cylinder.

The hose lines should then be relieved of pres­ sure by opening the torch needle valves and the working pressure regulator, one at a time, allowing the gas to escape. Again, it is a good practice to relieve the oxygen pressure and then the acetylene pressure. The hose should then be coiled or hung carefully to prevent damage or kinking.

(4) Soft soldering is used chiefly for copper, brass, and coated iron in combination with mechanical seams; that is, seams that are riv­ eted, bolted, or folded. It is also used where a leak-proof joint is desired, and sometimes for fitting joints to promote rigidity and prevent corrosion. Soft soldering is generally per­ formed only in very minor repair jobs. This process is used to join electrical connections because it forms a strong union with low elec­ trical resistance.

(a) Soft solder gradually yields under a steadily applied load and should not be used unless the transmitted loads are very low. It should never be used as a means of joining structural members.

(b) A soldering iron is the tool used in sol­ dering. Its purpose is to act as a source of heat for the soldering operation. The bit, or work­ ing face, is made from copper since this metal will readily absorb heat and transmit it to the work. Figure 4-33 shows a wedge-shaped bit.

FIGURE 4-33. Electric soldering iron.

(c) To tin the soldering iron, it is first heated to a bright red, and then the point is cleaned (by filing) until it is smooth and bright. No dirt or pits should remain on its surface. After the soldering iron has been mechanically cleaned, it should be reheated sufficiently to melt solder and chemically cleaned by rubbing it firmly on a block of sal ammoniac (ammo­ nium chloride). Rosin flux paste may also be used. Solder is then applied to the point and wiped with a clean cloth.

(d) A properly tinned copper iron has a thin unbroken film of solder over the entire surface of its point.

(e) Soft solders are chiefly alloys of tin and lead. The percentages of tin and lead vary considerably in various solder, with a corre­ sponding change in their melting points, rang­ ing from 145-311 °C (293-592 °F).

Half-and-half (50/50) solder is a general pur­ pose solder and is most frequently used. It contains equal proportions of tin and lead, and it melts at approximately 182 °C (360 °F).

(f) The application of the melted solder re­ quires somewhat more care than is apparent.

The parts to be soldered should be locked to­ gether or held mechanically or manually while tacking. To tack the seam, the hot copper iron is touched to a bar of solder, then the drops of solder adhering to the copper iron are used to tack the seam at a number of points. The film of solder between the surfaces of a joint must be kept thin to make the strongest joint.

(g) A hot, well-tinned soldering copper iron should be held so that its point lies flat on the metal (at the seam), while the back of the cop­ per iron extends over the seam proper at a 45-degree angle, and a bar of solder is touched to the point. As the solder Par 4-88 Page 4-61

Page 202Open in PDF

melts, the copper iron is drawn slowly along the seam. As much solder as necessary is added without raising the soldering copper iron from the job. The melted solder should run between the surfaces of the two sheets and cover the full width of the seam. Work should progress along the seam only as fast as the sol­ der will flow into the joint.

4-89. AIRCRAFT PARTS NOT TO BE WELDED.

a. Brace Wires and Cables. Do not weld aircraft parts whose proper function depends upon strength properties developed by coldworking. Among parts in this classification are streamlined wire and cables.

b. Brazed and Soldered Parts. Do not weld brazed or soldered parts as the brazing mixture or solder will penetrate and weaken the hot steel.

c. Alloy Steel Parts. Do not weld alloy steel parts such as aircraft bolts, turnbuckle ends, etc., which have been heat treated to improve their mechanical properties.

d. Nos. 2024 and 7075 Aluminum. Do not weld these two aluminum alloys (that are often used in aircraft construction) because the heat from the welding process will cause severe cracking. The 2024 aluminum is most often used in wing skins, fuselage skins, and in most structured airframe parts. The 7075 aluminum is most often used in machined fittings such as wing-spar attachments, landing-gear attach­ ments, and other structural parts.

4-90. WELDING ROD SELECTION.

Most aircraft repair shops that are prepared to make weld repairs should have the basic se­ lection of welding rods available. The best rods to stock, the metals they weld, and the AWS specification number are shown in ta­ ble 4-15.

4-91. REPAIR OF TUBULAR MEM­ BERS.

a. Inspection. Prior to repairing tubular members, carefully examine the structure sur­ rounding any visible damage to insure that no secondary damage remains undetected. Sec­ ondary damage may be produced in some structure, remote from the location of the pri­ mary damage, by the transmission of the dam­ aging load along the tube. Damage of this na­ ture usually occurs where the most abrupt change in direction of load travel is experi­ enced. If this damage remains undetected, subsequent normal loads may cause failure of the part.

b. Location and Alignment of Welds.

Unless otherwise noted, welded steel tubing may be spliced or repaired at any location along the length of the tube. To avoid distor­ tion, pay particular attention to the proper fit and alignment.

c. Members Dented at a Cluster. Repair dents at a steel-tube cluster joint by welding a specially formed steel patch plate over the dented area and surrounding tubes. (See fig­ ure 4-34.) To prepare the patch plate, cut a section of steel sheet of the same material and thickness as the heaviest tube damaged. Trim the reinforcement plate so that the fingers ex­ tend over the tubes a minimum of 1.5 times the respective tube diameter. (See figure 4-34.)

Remove all the existing finish on the damaged cluster-joint area to be covered by the rein­ forcement plate. The reinforcement plate may be formed before any welding is attempted, or it may be cut and tack-welded to one or more of the tubes in the cluster joint, then heated and formed around the joint to produce a smooth contour. Apply sufficient heat to the plate while forming so that there is generally a gap of no more than 1/16 inch from the con- Page 4-62 Par 4-88

Page 203Open in PDF

tour of the joint to the plate. In this operation formed by any two adjacent fingers of the avoid unnecessary heating, and exercise care to plate. After the plate is formed and tack prevent damage at the point of the angle welded to the cluster joint, weld all the plate edges to the cluster joint.

TABLE 4-15. Chart showing Welding Filler Rod selection.

Welding Rod # AMS Spec. AWS Spec. Welds these Metals 4130 4140 4043 308L 316L AZ61A ERTi-5 AMS 6457 AMS 6452 AMS 4190 AMS 5692 AMS 5692 AMS 4350 AMS 4954 AWS A5.18 AWS A5.28 AWS A5.10 AWS A5.9 AWS A5.9 AWS A5.19 AWS A5-16 Mild Steel, 4130 steel 4140 Steel Most weldable Aluminum 304 Stainless steel 316 Stainless steel AZ61A Magnesium Titanium Par 4-91 Page 4-63

Page 204OCROpen in PDF

LONGERON DENTED AT A STATION.

THICKNESS OF PATCH PLATE

SAME AS LONGERON THICKNESS.

PATCH PLATE BEFORE FORMING AND WELDING.

PATCH PLATE FORMED AND WELDED TO TUBES.

FIGURE 4-34. Finger patch repairs for members dented at a cluster.

Page 4-64 Par 4-91

Page 205Open in PDF

d. Members Dented in a Bay. R e p a i r dented, bent, cracked, or otherwise damaged tubular members by using a split-sleeve rein­ forcement. Carefully straighten the damaged member, and in the case of cracks, drill No. 40 (0.098) inch stop holes at the ends of the crack.

4-92. REPAIR BY WELDED SLEEVE.

This repair is outlined in figure 4-35. Select a length of steel tube sleeve having an inside di­ ameter approximately equal to the outside di­ ameter of the damaged tube and of the same material, and at least the same wall thickness.

Diagonally cut the sleeve reinforcement at a 30-degree angle on both ends so that the minimum distance of the sleeve from the edge of the crack or dent is not less than 1-1/2 times the diameter of the damaged tube. Cut through the entire length of the reinforcement sleeve, and separate the half-sections of the sleeve.

Clamp the two sleeve sections to the proper positions on the affected areas of the original tube. Weld the reinforcement sleeve along the length of the two sides, and weld both ends of the sleeve to the damaged tube. (See fig­ ure 4-35.) The filling of dents or cracks with welding rod in lieu of reinforcing the member is not acceptable.

4-93. REPAIR BY BOLTED SLEEVE.

Do not use bolted-sleeve repairs on welded steel-tube structure unless specifically author­ ized by the manufacturer or the FAA. The tube area removed by the bolt holes, in this type of repair, may prove critical.

4-94. WELDED-PATCH REPAIR. Dents or holes in tubing may be repaired by using a patch of the same material, one gauge thicker.

(See figure 4-36.)

a. Dented Tubing.

(1) Dents are not deeper than 1/10 of tube diameter, do not involve more than 1/4 of the tube circumference, and are not longer than tube diameter.

(2) Dents are free from cracks, abrasions, and sharp corners.

(3) The dented tubing can be substantially re­ formed, without cracking, before application of the patch.

b. Punctured Tubing. Holes are not longer than tube diameter and involve not more than 1/4 of tube circumference.

4-95. SPLICING TUBING BY INNER­ SLEEVE METHOD. If the damage to a structural tube is such that a partial replace­ ment of the tube is necessary, the inner-sleeve splice is recommended; especially where a smooth tube surface is desired. (See fig­ ure 4-37.)

a. Make a diagonal cut when removing the damaged portion of the tube, and remove the burr from the edges of the cut by filing or similar means. Diagonally cut a replacement steel tube of the same material and diameter, and at least the same wall thickness, to match the length of the removed portion of the dam­ aged tube. At each end of the replacement tube allow a 1/8-inch gap from the diagonal cuts to the stubs of the original tube. Select a length of steel tubing of the same material, and at least the same wall thickness, and of an out­ side diameter equal to the inside diameter of the damaged tube. Fit this inner-sleeve tube material snugly within the original tube, with a maximum diameter difference of 1/16 inch.

From this inner-sleeve tube material cut two sections of tubing, each of such a length that the ends of the inner sleeve will be a minimum distance of 1-1/2-tube diameters from the nearest end of the diagonal cut.

Par 4-91 Page 4-65

Page 206OCROpen in PDF

DENTED OR BENT TUBE

CRACKED TUBE

- REINFORCEMENT TUBE SPLIT NOTE:

LOCALLY DENTED OR

BENT MEMBERS SHOULD

FIRST BE REFORMED IN CLAMP.

REINFORCEMENT SLEEVE TO BE OF SAME

MATERIAL AND AT LEAST THE SAME GAUGE AS TUBE BEING REPAIRED.

1-1/2 A WELD 1-1/2 A

AS ALTERNATIVE TO SPLIT TUBE,

A TWO-PIECE REINFORCEMENT

SLEEVE MAY BE FORMED FROM STEEL SHEET OF THE SAME MATERIAL 30° AND AT LEAST THE SAME GAUGE AS - 1A → 1A - THE DAMAGED TUBE. USE FISHMOUTH +1-1/2A• 91-112

ENDS AND FOUR ROSETTE WELDS AS SHOWN.

FIGURE 4-35. Members dented in a bay (repairs by welded sleeve).

Page 4-66 Par 4-95

Page 207Open in PDF

FIGURE 4-36. Welded patch repair.

b. If the inner sleeve fits very tightly in the replacement tube, chill the sleeve with dry ice or cold water. If this is insufficient, polish down the diameter of the sleeve with emery cloth. Tack the outer and inner replacement tubes using rosette welds. Weld the inner sleeve to the tube stubs through the 1/8-inch gap, forming a weld bead over the gap.

4-96. SPLICING TUBING BY OUTER­ SLEEVE METHOD. If partial replacement of a tube is necessary, make the outer-sleeve splice using a replacement tube of the same di­ ameter. Since the outer-sleeve splice requires the greatest amount of welding, it should be used only when the other splicing methods are not suitable. Information on the replacement by use of the outer-sleeve method is given in figure 4-38 and figure 4-39.

a. Remove the damaged section of a tube utilizing a 90-degree cut. Cut a replacement steel tube of the same material, diameter, and at least the same wall thickness to match the length of the removed portion of the damaged tube. This replacement tube must bear against the stubs of the original tube with a total toler­ ance not to exceed 1/32 inch. The outer-sleeve tube material selected must be of the same material and at least the same wall thickness as the original tube. The clearance between inside diameter of the sleeve and the outside diameter of the original tube may not exceed 1/16 inch.

b. From this outer-sleeve tube material, cut diagonally (or fishmouth) two sections of tub­ ing, each of such length that the nearest end of the outer sleeve is a minimum distance of 1-1/2-tube diameters from the end of the cut on the original tube. Use a fishmouth sleeve wherever possible. Deburr the edges of the sleeves, replacement tube, and the original tube stubs.

c. Slip the two sleeves over the replacement tube, align the replacement tube with the origi­ nal tube stubs, and slip the sleeves over the center of each joint. Adjust the sleeves to suit the area and provide maximum reinforcement.

d. Tack weld the two sleeves to the re­ placement tube in two places before welding.

Apply a uniform weld around both ends of one of the reinforcement sleeves and allow the weld to cool; then, weld around both ends of the remaining reinforcement tube. Allow one sleeve weld to cool before welding the re­ maining tube to prevent undue warping.

Par 4-95 Page 4-67

Page 208Open in PDF

FIGURE 4-37. Splicing by inner-sleeve method.

4-97. SPLICING USING LARGER DI­ AMETER REPLACEMENT TUBES. The method of splicing structural tubes, as shown in figure 4-40, requires the least amount of cutting and welding. However, this splicing method cannot be used where the damaged tube is cut too near the adjacent cluster joints, or where bracket-mounting provisions make it necessary to maintain the same replacement tube diameter as the original. As an aid to in­ stalling the replacement tube, squarely cut the original damaged tube leaving a minimum short stub equal to 2-1/2-tube diameters on one end and a minimum long stub equal to 4-1/2-tube diameters on the other end. Select a length of steel tube of the same material and at least the same wall thickness, having an inside diameter approximately equal to the outside diameter of the damaged tube. Fit this re­ placement tube material snugly around the original tube with a maximum diameter differ­ ence of 1/16 inch. From this replacement tube material, cut a section of tubing diagonally (or fishmouth) of such a length that each end of the tube is a minimum distance of 1-1/2-tube diameters from the end of the cut on the origi­ nal tube. Use a fishmouth cut replacement tube wherever possible. Deburr the edges of the replacement tube and original tube stubs.

If a fishmouth cut is used, file out the sharp ra­ dius of the cut with a small round file.

Page 4-68 Par 4-97

Page 209OCROpen in PDF

30° SLEEVE 112-112- 30 ￾ A

ROSETTE WELDS MAY - WELD

BE OMITTED WHEN SLEEVES FIT TIGHTLY.

- REPLAGEMENT TUBE

ORIGINAL TUBE , FISH-MOUTH 1/2A- SLEEVE

- 1/2A 1/4A == = -A-

ROSETTE WELDS MAY WELD

BE OMITTED WHEN SLEEVES FIT TIGHTLY.

REPLACEMENT TUBE

ORIGINAL TUBE FOUR ROSETTE •WELD HERE FIRST ORIGINAL TUBE WELDS +1/4A

- 1/8" GAP +-1½A 7/24 1½A* FOR WELDING ALTERNATIVE SPLIT SLEEVE SPLICE ~ IF OUTSIDE DIAMETER OF ORIGINAL TUBE IS LESS THAN 1 INCH, SPLIT SLEEVE MAY BE MADE FROM STEEL TUBE OR SHEET STEEL. USE SAME MATERIAL OF AT LEAST THE SAME GAUGE.

FIGURE 4-38. Splicing by outer-sleeve method (replacement by welded outside sleeve).

Par 4-97 Page 4-69