AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 198–209
Page 210OCROpen in PDF

‹ ORIGINAL TUBE

SLEEVE SLEEVE TUBE +CY TUBE ń/4C 1/2B

ROSETTE ORIGINAL TUBE WELD WELD 1/4A LA- 30° 30 ORIGINAL TUBE 1/2A~ 112 SLEEVE HE GAP REPLACEMENT TUBE SLEEVE TUBE

TUBE BETWEEN SLEEVES FOR WELDING.

FIGURE 4-39. Tube replacement at a station by welded outer sleeves.

-2-1/2A REPLACEMENT TUBE 30° 30 ORIGINAL → 112A TUBE +1-1/2A→

- REPLACEMENT TUBE na

- 4-1/2A 30 · →112A ORIGINAL TUBE

•1-112A→ FIGURE 4-40. Splicing using larger diameter replacement tube.

Page 4-70 Par 4-97

Page 211Open in PDF

Spring the long stub of the original tube from the normal position, slip the replacement tube over the long stub, and then back over the short stub. Center the replacement tube be­ tween the stubs of the original tube. Tack weld one end of the replacement tube in sev­ eral places, then weld completely around the end. In order to prevent distortion, allow the weld to cool completely, then weld the re­ maining end of the replacement tube to the original tube.

4-98. REPAIRS AT BUILT-IN FUSE­ LAGE FITTINGS. Make splices in accor­ dance with the methods described in para­ graphs 4-86 through 4-92. Repair built-in fu­ selage fittings in the manner shown in fig­ ure 4-41. The following paragraphs outline the different methods as shown in figure 4-41.

a. Tube of Larger Diameter Than Origi­ nal. A tube (sleeve) of larger diameter than the original is used in the method shown in figure 4-41 (A). The forward splice is a 30-degree scarf splice. Cut the rear longeron (right) approximately 4 inches from the cen­ terline of the joint and fit a 1 inch long spacer over the longeron, and edge weld this spacer and longeron. Make a tapered “V” cut ap­ proximately 2 inches long in the aft end of the outer sleeve, and swage the end of the outer sleeve to fit the longeron and weld.

b. Tube of Same Diameter as Original. In the method shown in figure 4-41 (B) the new section is the same size as the longeron forward (left) of the fitting. The rear end (right) of the tube is cut at 30 degrees and forms the outside sleeve of the scarf splice. A sleeve is centered over the forward joint as in­ dicated.

c. Simple Sleeve. In figure 4-41 (C), it is as­ sumed the longeron is the same size on each side of the fitting. It is repaired by a sleeve of larger diameter than the longeron.

d. Large Difference in Longeron Diameter Each Side of Fitting. Figure 4-41 (D) as­ sumes that there is 1/4-inch difference in the diameter of the longeron on the two sides of the fitting. The section of longeron forward (left) of the fitting is cut at 30 degrees, and a section of tubing of the same size as the tube and of such length as to extend well to the rear (right) of the fitting is slipped through it. One end is cut at 30 degrees to fit the 30-degree scarf at left, and the other end fishmouthed.

This makes it possible to insert a tube of proper diameter to form an inside sleeve for the tube on the left of the fitting and an outside sleeve for the tube on the right of the fitting.

4-99. ENGINE-MOUNT REPAIRS. A l l welding on an engine mount must be of the highest quality, since vibration tends to ac­ centuate any minor defect. Engine-mount members should preferably be repaired by us­ ing a larger diameter replacement tube, tele­ scoped over the stub of the original member, and using fishmouth and rosette welds. How­ ever, 30-degree scarf welds in place of the fishmouth welds will be considered acceptable for engine-mount repair work.

a. Repaired engine mounts must be checked for accurate alignment. When tubes are used to replace bent or damaged ones, the original alignment of the structure must be maintained.

When drawings are not available, this can be done by measuring the distance between points of corresponding members that have not been distorted.

b. Grind out all cracked welds.

c. Use only high-grade metallurgically con­ trolled (mc) welding rods for engine-mount re­ pairs.

Par 4-97 Page 4-71

Page 212OCROpen in PDF

WELD SPACER APPROXIMATELY "A" LONG WELDED ON

INSIDE TUBE → 3A- (A) (B) GENERAL NOTE: -

ALL ROSETTE WELDS (C) TO BE & DIAMETER OF THE ORIGINAL TUBES.

GAP $"* 30° (D) FIGURE 4-41. Repairs at built-in fuselage fittings.

Page 4-72 Par 4-99

Page 213Open in PDF

d. If all members are out of alignment, re­ ject the engine mount and replace with one supplied by the manufacturer or one which was built to conform to the manufacturer’s draw­ ings. The method of checking the alignment of the fuselage or nacelle points should be re­ quested from the manufacturer.

e. Repair minor damage, such as a crack adjacent to an engine-attachment lug, by rew­ elding the ring and extending a gusset or a mounting lug past the damaged area. Enginemount rings which are extensively damaged must not be repaired, unless the method of re­ pair is specifically approved by the FAA, or the repair is accomplished in accordance with FAA-approved instructions.

f. If the manufacturer stress relieved the engine mount after welding it, the engine mount should be re-stress relieved after the weld repairs are made.

4-100. BUILT-UP TUBULAR WING OR TAIL-SPARS. Repair built-up tubular wing or tail-spars by using any of the applicable splices and methods of repair shown in fig­ ure 4-35 through figure 4-45, provided the spars are not heat treated. In the case of heattreated spars, the entire spar assembly would have to be reheat treated to the manufacturer’s specifications after completion of the repair.

In general, this will be found less practicable than replacing the spar with one furnished by the manufacturer or holder of the PMA for the part.

4-101. WING-BRACE STRUTS AND TAIL-BRACE STRUTS. In general, it will be found advantageous to replace damaged wing-brace struts made either from rounded or streamlined tubing with new members pur­ chased from the original manufacturer. How­ ever, there is no objection, from an airworthi­ ness point of view, to repairing such members in a proper manner. An acceptable method of repair, if streamlined tubing is used, will be found in figure 4-43. Repair similar members made of round tubes using a standard splice, as shown in figure 4-35, figure 4-37, or fig­ ure 4-38.

a. Location of Splices. Steel-brace struts may be spliced at any point along the length of the strut provided the splice does not overlap part of an end fitting. The jury-strut attach­ ment is not considered an end fitting; there­ fore, a splice may be made at this point. The repair procedure and workmanship minimize distortion due to welding and the necessity for subsequent straightening operations. Observe every repaired strut carefully during initial flights to ascertain that the vibration charac­ teristics of the strut and attaching components are not adversely affected by the repair. A wide range of speed and engine-power combi­ nation must be covered during this check.

b. Fit and Alignment. When making re­ pairs to wing and tail surface brace members, ensure to proper fit and alignment to avoid distortion.

4-102. LANDING GEAR REPAIR.

a. Round Tube Construction. R e p a i r landing gears made of round tubing using standard repairs and splices as shown in fig­ ure 4-35 and figure 4-41.

b. Streamline Tube Construction. R e p a i r landing gears made of streamlined tubing by either one of the methods shown in fig­ ure 4-42, figure 4-44, or figure 4-45.

c. Axle Assemblies. Representative types of repairable and nonrepairable landing gear axle assemblies are shown in figures 4-46 and 4-47.

The types as shown in A, B, and C of this fig­ ure are formed from steel tubing and may be repaired by the applicable method Par 4-99 Page 4-73

Page 214Open in PDF

A- Slot Width (Original Tube).

B- Outside Diameter (Insert Tube).

C- Streamline Tube Length of Major Axis.

S.L. Size A B C D 1” .375 .563 1.340 .496 1-¼ .375 .688 1.670 .619 1-½ .500 .875 2.005 .743 1-¾ .500 1.000` 2.339 .867 2 .500 1.125 2.670 .991 2-¼ .500 1.250 3.008 1.115 2-½ .500 1.375 3.342 1.239

ROUND INSERT TUBE (B) SHOULD BE AT LEAST OF SAME MATERIAL AND ONE GAUGE THICKER THAN ORIGINAL STREAMLINE TUBE (C).

FIGURE 4-42. Streamline tube splice using round tube (applicable to landing gear).

d. shown in figure 4-35 through figure 4-45.

However, it will always be necessary to ascer­ tain whether or not the members are heat treated. The axle assembly as shown in fig­ ure 4-47 is, in general, of a nonrepairable type for the following reasons.

(1) The axle stub is usually made from a highly heat-treated nickel alloy steel and care­ fully machined to close tolerances. These stubs are usually replaceable and must be re­ placed if damaged.

(2) The oleo portion of the structure is gen­ erally heat treated after welding, and is per­ fectly machined to ensure proper functioning of the shock absorber. These parts would be distorted by welding after machining.

4-103. REPAIRS TO WELDED ASSEM­ BLIES. These repairs may be made by the following methods.

a. A welded joint may be repaired by cut­ ting out the welded joint and replacing it with one properly gusseted. Standard splicing pro­ cedures should be followed.

Page 4-74 Par 4-102

Page 215Open in PDF

A- Minimum Length of Sleeve.

B- Streamline Tube Length of Minor Axis.

C- Streamline Tube Length of Major Axis.

S.L. Size A B C 1” 7.324 .572 1.340 1-¼ 9.128 .714 1.670 1-½ 10.960 .858 2.005 1-¾ 12.784 1.000 2.339 2 14.594 1.144 2.670 2-¼ 16.442 1.286 3.008 2-½ 18.268 1.430 3.342 FIGURE 4-43. Streamline tube splice using split sleeve (applicable to wing and tail surface brace struts and other members).

b. Replacing weld deposit by chipping out the metal deposited by the welding process and rewelding after properly reinforcing the joint by means of inserts or external gussets.

4-104. STAINLESS STEEL STRUC­ TURE. Repair structural components made from stainless steel, particularly the “18-8” va­ riety (18 percent chromium, 8 percent nickel), joined by spot welding, in accordance with the instructions furnished by the manufacturer, DER, or FAA. Substitution of bolted or riv­ eted connections for spot-welded joints are to be specifically approved by a DER or the FAA. Repair secondary structural and non­ structural elements such as tip bows or leading and trailing edge tip strips of wing and control surfaces by soldering with a 50-50 lead-tin sol­ der or a 60-40 lead-tin solder. For best results, use a flux of phosphoric acid (syrup). Since the purpose of flux is to attack the metal so that the soldering will be effective, remove ex­ cess flux by washing the joint. Due to the high-heat conductivity of the stainless steel, use a soldering iron large enough to do the work properly.

Par 4-103 Page 4-75

Page 216Open in PDF

INSERT TUBE IS OF SAME STREAMLINE TUBING AS ORIGINAL.

A- Is ²/³ B.

B- Is Minor Axis Length of Original Streamline Tube.

C- Is Major Axis Length of Original Streamline Tube.

S.L. Size A B C L 1” .382 .572 1.340 5.160 1-¼ .476 .714 1.670 6.430 1-½ .572 .858 2.005 7.720 1-¾ .667 1.000 2.339 9.000 2 .763 1.144 2.670 10.300 2-¼ .858 1.286 3.008 11.580 2-½ .954 1.430 3.342 12.880 FIGURE 4-44. Streamline tube splice using split insert (applicable to landing gear).

Page 4-76 Par 4-104

Page 217Open in PDF

A- Streamline Tube Length of Minor Axis, Plate Widths.

B- Distance of First Plate From Leading Edge, ²/³ A.

C- Streamline Tube Length of Major Axis.

S.L. Size A B C 6A 1” .572 .382 1.340 3.430 1-¼ .714 .476 1.670 4.280 1-½ .858 .572 2.005 5.150 1-¾ 1.000 .667 2.339 6.000 2 1.144 .762 2.670 6.860 2-¼ 1.286 .858 3.008 7.720 2-½ 1.430 .954 3.342 8.580 FIGURE 4-45. Streamline tube splice using plates (applicable to landing gear).

Par 4-104 Page 4-77

Page 218Open in PDF

FIGURE 4-46. Representative types of repairable axle assemblies.

Page 4-78 Par 4-104

Page 219Open in PDF

FIGURE 4-47. Landing gear assemblies that CANNOT be repaired by welding.

4-105.  4-110. [RESERVED.] Par 4-104 Page 4-79 (and 4-80)

Page 220Open in PDF

SECTION 6. WELDING AND BRAZING SAFETY

4-111. GENERAL. A number of inherent hazards exist in the use of oxy-fuel welding and cutting apparatus. It is necessary that proper safety and operating procedures are un­ derstood. A thorough understanding of the proper safety and operating procedures mini­ mizes the hazards involved and adds to the pleasure and efficiency of your work.

4-112. FIRE AND EXPLOSION SAFETY.

Fires occur in welding areas because flamma­ bles are left where they can be ignited by welding sparks or gas welding flames. Before welding, clear the welding area of all flamma­ bles such as rags, paper, wood, paint cans, sol­ vent, and trash containers. Do not weld in ar­ eas where flammables are present.

a. Unless absolutely necessary, never weld any tank or radiator that has had a flam­ mable in it, including gasoline, av-gas, motor oil, hydraulic fluid, or any other liquid that could ignite if the vapor and temperature reach a flashpoint. Explosions often occur when empty tanks are being welded or cut open with a torch.

b. If welding such tanks or radiator cool­ ers is absolutely necessary, the tank must first be washed with a caustic-based, water-soluble liquid, rinsed with plenty of clear water, and then dried. Before welding, the tank or con­ tainer should be thoroughly purged with argon, or other inert gas, while the welding is in proc­ ess.

4-113. WELDING WORK AREA.

a. The work area must have a fireproof floor, concrete floors are recommend.

b. Use heat-resistant shields to protect nearby walls or unprotected flooring from sparks and hot metal.

c. Maintain an adequate suction ventilation system to prevent the concentration of oxygen/fuel gas, flammable gases, and/or toxic fumes. It is important to remember that oxy­ gen will not burn. The presence of oxygen, however, serves to accelerate combustion, and causes materials to burn with great intensity.

CAUTION: Oil and grease in the presence of oxygen can ignite and burn violently.

d. A completely clean welding shop area with white walls, ceiling, and floor; and with plenty of light, is better for welding. The bet­ ter the lighting conditions, the easier it is to see the weld puddle and make excellent aircraftquality welds.

e. During oxy-fuel processes use work benches or tables with fireproof tops. Fire bricks commonly top these surfaces and sup­ port the work.

f. Chain or otherwise secure oxygen and fuel gas cylinders to a wall, bench, post, cylin­ der cart, etc. This will protect them from fal­ ling and hold them upright.

4-114. FIRE PROTECTION. Practice fire prevention techniques whenever oxy-fuel op­ erations are in progress. Simple precautions prevent most fires, and minimize damage in the event a fire does occur. Always practice the following rules and safety procedures.

Par 4-111 Page 4-81

Page 221Open in PDF

a. Inspect oxy-fuel apparatus for oil, grease, or damaged parts. DO NOT use the oxy-fuel apparatus if oil or grease is present or if damage is evident. Have the oxy-fuel appa­ ratus cleaned and/or repaired by a qualified re­ pair technician before it is used.

b. Never use oil or grease on or around any oxy-fuel apparatus. Even a trace of oil or grease can ignite and burn violently in the presence of oxygen.

c. Keep flames, heat, and sparks away from cylinders and boxes.

d. Flying sparks can travel as much as 35 feet. Move combustibles a safe distance away from areas where oxy-fuel operations are performed.

e. Use approved heat-resistant shields to protect nearby walls, floor, and ceiling.

f. Have a fire extinguisher of the proper class (ABC) and size in the work area. Inspect it regularly to ensure that it is in proper work­ ing order. Know how it is used.

g. Use oxy-fuel equipment only with the gases for which it is intended.

h. DO NOT open an acetylene cylinder valve more than approximately 1-1/2 turns and preferably no more than 3/4 of a turn. Keep the cylinder wrench, if one is required, on the cylinder valve so, if necessary, the cylinder may be turned off quickly.

i. On all gases except acetylene, open the cylinder valve completely to seal the cylinder back-seal packing.

j. Never test for gas leaks with a flame.

Use an approved leak-detector solution.

k. When work is complete , inspect the area for possible fires or smoldering materials.

l. Special care should be taken when welding structural tubing that has been coated on the inside with linseed oil. Smoke and fire may be generated by the heat of the torch. En­ sure that an observer with a fire extinguisher is close.

4-115. PROTECTIVE APPAREL.

a. Protect yourself from sparks, flying slag, and flame brilliance at all times.

(1) For gas welding and brazing, use number 3 or 4 green-shaded tempered lenses.

(2) When gas welding aluminum, use cobalt-blue tint lenses.

(3) When arc welding, including TIG, MIG, and plasma cutting; use number 9 to 12 green lenses and a full face-and-neck cov­ ering helmet.

(4) Electronically darkening lenses pro­ vide number 3 to 12 automatic darkening as soon as the arc is ignited.

b. Wear protective gloves, sleeves, aprons, and lace-up shoes to protect skin and clothing from sparks and slag.

CAUTION: Keep all clothing and protective apparel absolutely free of oil or grease.

4-116. FIRST-AID KITS. Always keep a special welder’s first-aid kit where it is easily accessible. Burns are the most common welding accidents.

4-117.  4-128. [RESERVED.] Page 4-82 Par 4-107