AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 265–276
Page 277Open in PDF

6-14. CONCENTRATION CELL COR- ROSION. Concentration cell corrosion, (also known as Crevice Corrosion) is corrosion of metals in a metal-to-metal joint, corrosion at the edge of a joint even though the joined met­ als are identical, or corrosion of a spot on the metal surface covered by a foreign material.

Metal ion concentration cells and oxygen con­ centration cells are the two general types of concentration cell corrosion. (See figure 6-6.)

a. Metal Ion Concentration Cells . The solution may consist of water and ions of the metal which is in contact with water. A high concentration of the metal ions will normally exist under faying surfaces where the solution is stagnant, and a low concentration of metal ions will exist adjacent to the crevice which is created by the faying surface. An electrical potential will exist between the two points; the area of the metal in contact with the low con­ centration of metal ions will be anodic and corrode, and the area in contact with the high metal ion concentration will be cathodic and not show signs of corrosion.

b. Oxygen Concentration Cells. T h e solution in contact with the metal surface will normally contain dissolved oxygen. An oxy­ gen cell can develop at any point where the oxygen in the air is not allowed to diffuse into the solution, thereby creating a difference in oxygen concentration between two points.

Typical locations of oxygen concentration cells are under gaskets, wood, rubber, and other materials in contact with the metal sur­ face. Corrosion will occur at the area of low oxygen concentration (anode). Alloys such as stainless steel are particularly susceptible to this type of crevice corrosion.

6-15. ACTIVE-PASSIVE CELLS. Metals which depend on a tightly adhering passive film, usually an oxide, for corrosion protection are prone to rapid corrosive attack by activepassive cells. Active-passive cells are often re­ ferred to as a type of concentration cell corro­ sion. However, the active-passive cell is actu­ ally two forms of corrosion working in con­ junction. The corrosive action usually starts as an oxygen concentration cell. As an example, salt deposits on the metal surface in the pres­ ence of water containing oxygen can create the oxygen cell. The passive film will be broken beneath the salt crystals. Once the passive film is broken, the active metal beneath the film will be exposed to corrosive attack. (See figure 6-7.) Rapid pitting of the active metal will result. This reaction can become locally intense due to several factors. First the reac­ tion is augmented by the affected area, since the proportion of the exposed base metal is small compared to the surrounding non­ reactive metal. This effectively concentrates the focal point of the reaction, often resulting in deep pits in a short time and a greater rate of corrosion.

FIGURE 6-6. Concentration cell corrosion.

Page 6-6 Par 6-14

Page 278Open in PDF

6-16. FILIFORM CORROSION. Filiform corrosion is a special form of oxygen concen­ tration cell which occurs on metal surfaces having an organic coating system. It is recog­ nized by its characteristic worm-like trace of corrosion products beneath the paint film.

(See figure 6-8.) Polyurethane finishes are es­ pecially susceptible to filiform corrosion. Fili­ form occurs when the relative humidity of the air is between 78 and 90 percent and the sur­ face is slightly acidic. This corrosion usually attacks steel and aluminum surfaces. The traces never cross on steel, but they will cross under one another on aluminum which makes the damage deeper and more severe for alumi­ num. If the corrosion is not removed, the area treated, and a protective finish applied, the cor­ rosion can lead to inter-granular corrosion, es­ pecially around fasteners and at seams. Fili­ form corrosion can be removed using glass bead blasting material with portable abrasive blasting equipment or sanding. Filiform corro­ sion can be prevented by storing aircraft in an environment with a relative humidity below 70 percent, using coating systems having a low rate of diffusion for oxygen and water vapors, and by washing the aircraft to remove acidic contaminants from the surface.

6-17. INTERGRANULAR CORROSION.

Inter-granular corrosion is an attack on the grain boundaries of a metal. A highly magni­ fied cross section of any commercial alloy shows the granular structure of the metal. It consists of quantities of individual grains, and each of these tiny grains has a clearly FIGURE 6-8. Filiform corrosion.

defined boundary which chemically differs from the metal within the grain. The grain boundary and the grain center can react with each other as anode and cathode when in con­ tact with an electrolyte. (See figure 6-9.)

Rapid selective corrosion of the grain bounda­ ries can occur. High-strength aluminum alloys such as 2014 and 7075 are more susceptible to inter-granular corrosion if they have been im­ properly heat-treated and then exposed to a corrosive environment.

6-18. EXFOLIATION CORROSION. Exfoliation corrosion is an advanced form of in­ ter-granular corrosion and shows itself by lift­ ing up the surface grains of a metal by the force of expanding corrosion products occur­ ring at the grain boundaries just below the sur­ face. (See figure 6-10.) It is visible evidence of inter-granular corrosion and is most often seen on extruded sections where grain thick­ ness are usually less than in rolled forms.

FIGURE 6-7. Active-passive cell.

Par 6-16 Page 6-7

Page 279Open in PDF

FIGURE 6-9. Inter-granular Corrosion of 7075-T6 aluminum adjacent to steel fastener.

FIGURE 6-10. Exfoliation corrosion.

6-19. GALV ANIC CORROSION. Gal­ vanic corrosion occurs when two dissimilar metals make contact in the presence of an electrolyte. (See figure 6-11.) It is usually recognizable by the presence of a build-up of corrosion at the joint between the metals.

6-20. STRESS CORROSION CRACKING .

This form of corrosion involves a constant or cyclic stress, acting in conjunction with a damaging chemical environment. The stress may be caused by internal or external loading.

a. Internal stress may be trapped in a part of structure during manufacturing proc­ esses such as cold working or by unequal cooling from high temperatures. Most manu­ facturers follow up these processes with a stress relief operation. Even so, sometimes stress remains trapped. The stress may be ex­ ternally introduced in part structure by rivet­ ing, welding, bolting, clamping, press fit, etc.

If a slight mismatch occurs, or a fastener is over-torque, internal stress will be present.

b. Internal stress is more important than design stress, because stress corrosion is diffi­ cult to recognize before it has overcome the design safety factor. The level of stress varies from point to point within the metal. Stresses near the yield strength are generally necessary to promote stress corrosion cracking. (See fig­ ure 6-12.) However, failures may occur at lower stresses. Specific environments have been identified which cause stress corrosion cracking of certain alloys.

Page 6-8 Par 6-18

Page 280Open in PDF

FIGURE 6-11. Galvanic corrosion of magnesium adjacent to steel fastener.

FIGURE 6-12. Stress corrosion cracking.

(1) Salt solutions and sea water cause stress corrosion cracking of high-strength, heat-treated steel and aluminum alloys.

(2) Methyl alcohol-hydrochloric acid solutions will cause stress corrosion cracking of some titanium alloys.

(3) Magnesium alloys may stresscorrode in moist air.

(4) Stress Corrosion may be reduced by

• applying protective coatings,

• stress relief heat treatments,

• using corrosion inhibitors, or

• controlling the environment.

6-21. FATIGUE CORROSION . Fatigue corrosion involves cyclic stress and a corrosive environment. Metals may withstand cyclic stress for an infinite number of cycles so long as the stress is below the endurance limit of the metal. Once the limit has been exceeded, the metal will eventually crack and fail from metal fatigue. However, when the part or structure undergoing cyclic stress is also exposed to a corrosive environment, the stress level for fail­ ure may be reduced many times. Thus, failure occurs at stress levels that can be dangerously low depending on the number of cycles as­ signed to the life-limited part.

a. Fatigue corrosion failure occurs in two stages. During the first stage the combined action of corrosion and cyclic stress damages the metal by pitting and crack formations to such a degree that fracture by cyclic stress will occur, even if the corrosive environment is completely removed.

b. The second stage is essentially a fa­ tigue stage in which failure proceeds by propa­ gation of the crack (often from a corrosion pit or pits). It is controlled primarily by stress concentration effects and the physical proper­ ties of the metal. Fracture of a metal part due to fatigue corrosion, generally occurs Par 6-20 Page 6-9

Page 281Open in PDF

at a stress level far below the fatigue limit of an uncorroded part, even though the amount of corrosion is relatively small.

6-22. FRETTING CORROSION. Fretting corrosion,(also known as wear corrosion or friction oxidation) can occur at the interface of two highly-loaded surfaces which are not sup­ posed to move against each other. However, vibration may cause the surfaces to rub to­ gether resulting in an abrasive wear known as fretting. (See figure 6 -13.) The protective film on the metallic surfaces is removed by this rubbing action. With continued rubbing, metal particles sheared from the surface of the metal combine with oxygen to form metal ox­ ide. As these oxides accumulate, they cause damage by abrasive action and increased local stress. The most common example of fretting corrosion is the smoking rivet found on engine cowling and wing skins. This is one corrosion reaction that is not driven by an electrolyte, and in fact, moisture may inhibit the reaction.

Application of a lubricant or installation of a fretting-resistant material between the two sur­ faces can reduce fretting corrosion.

FIGURE 6-13. Fretting corrosion.

6-23.  6-28. [RESERVED.] Page 6-10 Par 6-21

Page 282Open in PDF

SECTION 3. CORROSION PROTECTION MEASURES FOR BASIC MATERIALS

6-29. GENERAL. In the repair of aircraft, apply corrosion proofing of the same type or equivalent to that originally applied unless the repair would result in increased susceptibility to corrosion, in which case use additional cor­ rosion protection measures. The following is a list of the most commonly-used corrosionproofing techniques.

6-30. ANODIZING AND RELATED PROCESSES. In anodizing, aluminum alloys are placed in an electrolytic bath causing a thin film of aluminum oxide to form on the surface of the aluminum. This is resistant to corrosion and affords a good paint base. However, other processes, which do not provide as good a cor­ rosive protection as anodizing, are good paint bases. The processes are:

a. Alkaline cleaning followed by chromic acid dip;

b. Alcoholic phosphoric acid cleaner; and

c. Alkaline dichromate treatment.

6-31. PLATING. Steels are commonly plated with other metals to prevent corrosion.

Plating is accomplished by placing the article in an electrolytic bath. Metals used in plating vary in the corrosion protection they afford steel. For instance, in platings that corrode be­ fore steel, such as zinc or cadmium, slight breaks or cracks throughout the plating will not result in rusting of the exposed steel. With the surface metal corroded, the steel is pro­ tected. However, when the steel corrodes faster than the plate metal, such as chromium, the amount of protection depends on the tight­ ness of the plating. Post-plate bake treatment to relieve hydrogen embrittlement is a neces­ sary part of replating procedures for high-strength steel parts. High-strength nuts and bolts are susceptible to failure from hydro­ gen embrittlement. Because of the potential failures of embrittled parts, careful control over the heat treatment, grinding, preplate cleaning, plating, and post-plate baking of high-strength parts is necessary.

6-32. PHOSPHATE RUST-PROOFING .

This process is commercially known as Parkerizing, Bonderizing, Granodizing, etc.

The coating placed on the part is used to pro­ tect steel parts after machining and before painting.

6-33. CHROME-PICKLE TREATMENT.

Magnesium parts which have been immersed or brushed with a solution of nitric acid and sodium dichromate will be protected for tem­ porary storage. The coating will also serve as a bond for subsequent organic finishes. Sealed chrome-pickle treatment is used on magnesium parts for long term protection. Diluted chro­ mic acid is a touch-up treatment. It is less critical to apply and can be applied over previ­ ously-applied thin chromate films.

6-34. DICHROMATE TREATMENT.

This treatment consists of boiling magnesium parts in a solution of sodium dichromate. It provides good paint base and protective quali­ ties on all standard wrought magnesium alloys except the magnesium-thorium alloys. Acid pickling of the magnesium surface prior to ap­ plication of the dichromate treatment is re­ quired if maximum corrosion resistance of the finish is expected.

6-35. STANNATE IMMERSION TREAT- MENT. Stannate immersion treatment deposits a layer of tin. It is a protective paint base for magnesium alloy parts which contain inserts and fasteners of a dissimilar metal such as Par 6-29 Page 6-11

Page 283Open in PDF

brass, copper, or steel. This treatment cannot be used with parts containing aluminum inserts or fasteners because the high alkalinity of the bath attacks the aluminum.

6-36. GALV ANIC ANODIZING TREAT- MENT. An electrolytic process that provides a paint base and corrosion-preventive film on magnesium alloys containing manganese.

6-37. CLADDING . Aluminum alloys which are susceptible to corrosion are frequently clad with pure aluminum. Slight pits, scratches, or other defects through the cladding material must be avoided, since the aluminum alloy core will corrode rapidly.

6-38. METAL SPRAYING . Metal is melted and sprayed on the surface to be protected.

The surface must be properly prepared and thoroughly cleaned to prevent peeling of the sprayed coat.

6-39. SHOT-PEENING . Shot-peening and other treatments, by which the surface can be placed in compression, are effective in pre­ venting stress corrosion.

6-40. ORGANIC COATINGS. Zinc chro­ mate primer, enamels, chlorinated rubber com­ pounds, etc., are organic coatings commonly used to protect metals.

6-41. DOPE PROOFING. When doped fabrics are applied over an organic finished metal structure, the dope will have a tendency to loosen the finish on the metal. For this rea­ son, organic coatings on the metal are usually covered with a dope-proof paint, with metal foil, or with cellulose tape to prevent the dope from soaking through.

6-42. TUBE INTERIORS. Protect the inte­ riors of structural steel and aluminum tubing against corrosion. A small amount of water entrapped in a tube can corrode entirely through the tube thickness in a short period.

Coat the tube interior by flushing with hot lin­ seed oil, paralketone, or other approved corro­ sion inhibitor. The flushing liquid is usually introduced through small holes drilled in the tubing. Allow the flushing liquid to drain and plug the holes with a screw or by other means to prevent entry of moisture. Air and water­ tight sealing of the tubing will also give ade­ quate protection against corrosion if the tubing is internally dry before being sealed.

6-43.  6-49. [RESERVED.] Page 6-12 Par 6-35

Page 284Open in PDF

SECTION 4. CORROSION PREVENTIVE MAINTENANCE

6-50. GUIDELINES: ALL AIRCRAFT.

Corrosion prevention depends on a compre­ hensive prevention and control plan, imple­ mented from the start of operation of an air­ craft, which includes:

a. Adequately-trained personnel in

(1) recognition of corrosion-inducing conditions;

(2) corrosion identification techniques;

(3) corrosion detection, cleaning, and treating; and

(4) lubrication and preservation of air­ craft structure and components.

b. Inspection for corrosion on a sched­ uled basis.

c. Thorough cleaning , inspection, lubri­ cation, and preservation at prescribed intervals.

d. Prompt corrosion treatment after de­ tection.

e. Accurate record-keeping and report­ ing of material or design deficiencies to the manufacturer and the Federal Aviation Ad­ ministration (FAA).

f. Use of appropriate materials , equip­ ment, and technical publications.

g. Maintenance of the basic finish sys­ tems.

h. Keeping drain holes and passages open and functional. Sealants, leveling com­ pounds, miscellaneous debris, or corrosion in­ hibitors should not block drain paths.

i. Replacing deteriorated or damaged gaskets and sealants (using non-corrosive type sealants) to avoid water intrusion and entrap­ ment that leads to corrosion.

j. Minimizing the exposure of aircraft to adverse environments by keeping the aircraft in a hangar.

k. Periodic and frequent inspection of areas where there are foamed plastics or other absorbent material.

l. Daily draining of fuel cavities to re­ move accumulated water and other foreign matter.

m. Daily wipe-down of exposed critical surfaces of hydraulic cylinders.

6-51. GUIDELINES: AIRCRAFT OP - ERATING OVER SALT WATER. In addi­ tion to the inspection and treatment prescribed above, the following treatment shall be ap­ plied:

a. Remove all traces of salt water and salt water residue by thoroughly washing the air­ craft with fresh water.

(1) After drying, coat the propeller, hubs, blades and other unpainted or unpro­ tected parts of the engine and its installation parts by spraying or rubbing lightly with corro­ sion preventive compound, Specification MIL-C-16173, Grade 4.

(2) Apply this mixture on parts that move or require some lubrication and on all fittings subject to corrosion such as landing gear retracting plungers, control surface hinges, control cables, exposed rivets and bolts, and other similar parts not protected by Par 6-50 Page 6-13

Page 285Open in PDF

paint. Apply with a cloth or a soft brush soaked in the mixture.

(3) Wipe off excess mixture. When ap­ plying the mixture take care that as little as possible is deposited on exhaust pipes or col­ lector rings to avoid a fire hazard when the en­ gine is started. Keep the ignition wires, pro­ peller anti-icer feed hose, tires, and other rub­ ber parts free of the mixture.

b. Where maximum corrosion protection is desired on stationary parts, use exterior sur­ face corrosion preventive compound, Specifi­ cation MIL-C-16173, grade I.

c. Wipe the exposed portion of the land­ ing gear shock strut piston with a cloth soaked in the applicable hydraulic fluid.

d. Most parts of landing gear wheels are made from magnesium or aluminum alloys which corrode rapidly unless carefully pro­ tected. When the aircraft operates near salt water and off coral beaches, the corrosion can be very rapid. Inspect wheels to determine the paint condition.

e. Refinish portions of a wheel where paint has deteriorated, peeled, or chipped.

f. Except for friction and bearing sur­ faces, apply a protective coating to all parts of wheels and brake assemblies.

6-52.  6-62. [RESERVED.] Page 6-14 Par 6-51

Page 286Open in PDF

SECTION 5. VISUAL CORROSION INSPECTION GUIDE FOR AIRCRAFT

6-63. GENERAL. This guide provides a general inspection checklist for those parts or surfaces that can be visually inspected without disassembly of the aircraft. It is intended for use in establishing corrosion inspection areas for which the manufacturer has not provided a recommended corrosion inspection program.

The manufacturer’s recommended corrosion inspection program will take precedence over this guideline. These inspections should be accomplished in conjunction with other pre­ ventive maintenance.

6-64. EXHAUST TRAIL AREAS.

a. Visually inspect paint in areas of the exhaust trails for damage.

b. Visually inspect under fairings, around rivet heads, and in skin crevices, for corrosion in areas of engine exhaust trail.

6-65. BATTERY COMPARTMENTS AND BATTERY VENT OPENINGS.

a. Inspect battery compartment for electrolyte spillage, corrosion, and condition of protective paint.

b. Inspect area around battery vent for corrosion.

6-66. LAVATORIES AND GALLEYS.

Inspection areas around lavatories, sinks, and ranges for spillage and corrosion. Pay par­ ticular attention to floor area and the area be­ hind and under lavatories, sinks, and ranges.

6-67. BILGE AREAS.

a. Inspect bilge areas for waste hydraulic fluids, water, dirt, loose fasteners, drill chips, and other debris.

b. Remove any foreign material from bilge and inspect for corrosion.

6-68. WHEEL WELLS AND LANDING GEAR. Inspect wheel well area and landing gear components for damage to exterior finish coating and corrosion. Particular attention should be given to exposed surfaces of struts, oleos, arms, links, and attaching hardware;

axle interiors, exposed position indicator switches and other electrical equipment; crev­ ices between stiffeners, ribs, and lower skin surfaces; magnesium wheels, particularly around bolt heads, lugs, and wheel web areas;

and exposed rigid tubing at “B” nuts and fer­ rules under clamps, and tubing identification tapes.

6-69. EXTERNAL SKIN AREAS.

a. Inspect external skin surfaces for damage to protective finishes and corrosion.

b. Inspect around fasteners for damage to protective finishes and corrosion.

c. Inspect lap joints for bulging of skin surface, which may indicate the presence of corrosion between the faying surfaces. Skin cracks and/or dished or missing fastener heads may also indicate severe corrosion in bonded joints.

d. Inspect area around spot welds for bulges, cracks, or corrosion.

e. Inspect piano type hinges for corro­ sion. When piano hinges are inspected they should be lubricated and actuated through sev­ eral cycles to ensure complete penetration of the lubricant.

Par 6-63 Page 6-15

Page 287Open in PDF

f. Inspect thick alloy skin surfaces for pitting, intergranular corrosion, and exfoliation of the metal. Look for white or gray deposits around countersunk fastener heads and raised areas or bumps under the paint film.

g. Inspect composite skins for corrosion of attachment fasteners.

6-70. WATER ENTRAPMENT AREAS.

Inspect area around edge of drain holes for cor­ rosion and ensure that drain holes are not blocked by debris.

6-71. ENGINE FRONTAL AREAS.

a. Inspect reciprocating engine cylinder fins, engine cases, and cooling air ducts for damage to exterior finish and corrosion.

b. Inspect radiator cooler cores for cor­ rosion.

6-72. ELECTRONIC PACKAGE COM - PARTMENTS.

a. Inspect circuit-breakers, contact points, and switches for evidence of moisture and corrosive attack.

b. Treatment of corrosion in electrical and electronic components should be done by or supervised by qualified personnel familiar with the function of the unit involved.

6-73. FLEXIBLE HOSE ASSEMBLIES.

a. Inspect hose assemblies for chafing, weather-checking, hardening, discoloration, evidence of fungus, torn weather protective coatings or sleeves, and corrosion of fittings.

b. Replace any defective, damaged, twisted, or bulging hoses.

6-74. SANDWICH PANELS. Inspect edges of sandwich panels for damage to the corrosion protection finish or sealant and for corrosion.

6-75. CONTROL CABLES.

a. Inspect control cables for bare spots in the preservative coating and corrosion.

b. If external corrosion is found, relieve tension on the cable and check internal strands for corrosion. Cables with corrosion on inter­ nal strands should be replaced. External cor­ rosion should be removed by a clean, dry, coarse rag or fiber brush. A preservative should be applied after removal of external corrosion.

6-76. INTEGRAL FUEL CELLS.

a. Inspect top coat finish for breaks, peeling, lifting of surface, or other damage.

b. Inspect aircraft structure for top coat finish damage from pitting or intergranular corrosion.

6-77. ELECTRICAL CONNECTORS.

a. Inspect electrical connectors for breaks in potting compound and corrosion of pins and wires.

b. If the electrical connector is suspected of having moisture intrusion, disas­ semble the connector, clean the connector, and inspect it for corrosion.

6-78.  6-88. [RESERVED.] Page 6-16 Par 6-69

Page 288Open in PDF

SECTION 6. CORROSION REMOVAL PROCEDURES

6-89. GENERAL. General safety precau­ tions for handling materials with hazardous physical properties are outlined in the follow­ ing paragraphs. They also address emergency procedures for immediate treatment of person­ nel who have inadvertently come into contact with harmful materials. All personnel respon­ sible for using or handling hazardous materials should be thoroughly familiar with the infor­ mation in the following paragraphs.

6-90. SAFETY PRECAUTIONS.

a. Chemical. When required to use or handle solvents, special cleaners, paint strip­ pers (strong alkalies and acids), etchants (cor­ rosion removers containing acids), or surface activation material (Alodine 1200), observe the following safety precautions:

(1) Avoid prolonged breathing of sol­ vent or acid vapors.

(2) Never add water to acid. Always add acid to water.

(3) Mix all chemicals per the manufac­ turer’s instructions.

(4) Clean water for emergency use should be available in the immediate work area before starting work.

(5) Avoid prolonged or repeated contact with the skin of solvents, cleaners, etchants (acid), or conversion coating material (Alodine solution). Rubber or plastic gloves should be worn. Goggles or plastic face shields and suit­ able protective clothing should be worn when cleaning, stripping, etching, or conver­ sion coating overhead surfaces.

(6) When mixing alkalies with water or other substance, use containers that are made to withstand heat generated by this process.

(7) Wash any paint stripper, etchant, or conversion coating material immediately from body, skin, or clothing.

(8) Materials splashed into the eyes should be promptly flushed out with water, and medical aid obtained immediately.

(9) Do not eat or keep food in areas where poisons may be absorbed. Always wash hands before eating or smoking.

(10) Verify that the area within 50 feet of any cleaning or treating operations where low flash point (140 °F or below) materials are being used, is clear and remains clear of all potential ignition sources.

(11) Suitable fire-extinguishing equip­ ment should be available to the clean­ ing/treating area.

(12) Equipment should be effectively grounded where any flammable materials are being used.

(13) If materials (acid, alkali, paint re­ mover, or conversion coatings) are spilled on equipment and/or tools, treat immediately by rinsing with clean water, if possible, and /or neutralizing acids with baking soda and alka­ lies with a weak (5 percent) solution of acetic acid in water.

Par 6-89 Page 6-17