AC 43.13-1B

Change 1Historical

Advisory circular · Acceptable Methods, Techniques, and Practices—Aircraft Inspection and Repair

A newer version is currentThis is a historical version. AC 43.13-1B CHG 1 Ed Update is the version in force, approved September 27, 2001.
Approved
September 9, 1998
Last reviewed
June 11, 2024
Cancels
AC43.13-1B
Family
AC 43.13-1 · 7 versions
Revision
B, change 1
14 CFR parts
43, 65, 145, 21, 105, 23, 91, 121, 25
Cited by
95 ADs

Guidance, not mandatory unless a rule or AD requires it. DRS record last changed November 21, 2025.

Show pages 277–288
Page 289Open in PDF

(14) In confined location, do not use solvents with a low flash point, (below 100 �F) such as Methyl Ethyl Ketone (MEK) and ace­ tone.

(15) All equipment should be cleaned after work has been completed.

(16) Check and follow all applicable re­ strictions and requirements on the use of sol­ vents, primers, and top coats.

(17) Check and follow all applicable re­ strictions and requirements for use and dis­ posal of waste material.

b. Blasting. The following precautions should be taken when using any type of blast­ ing equipment:

(1) Operators should be adequately protected with complete face and head cover­ ing equipment, and provided with pure breathing air.

(2) Static-ground the dry abrasive blaster and the material to be blasted.

(3) Magnesium cuttings and small shavings can ignite easily and are an extreme hazard. Fires of this metal must be extin­ guished with absolutely dry talc, calcium car­ bonate, sand, or graphite by applying the pow­ der to a depth of 1/2 inch over the metal.

(4) Titanium alloys and high-tensile­ strength steel create sparks during dry abrasive blasting. Care should be taken to ensure that hazardous concentrations of flammable vapors do not exist.

6-91. CORROSION CONTROL WORK PROCEDURES. The effectiveness of corro­ sion control depends on how well basic work procedures are followed. The following com­ mon work practices are recommended:

a. If rework procedures or materials are unknown, contact the aircraft manufacturer or FAA authorized Designated Engineering Rep­ resentative (DER) before proceeding.

b. The work areas , equipment, and com­ ponents should be clean and free of chips, grit, dirt, and foreign materials.

c. Do not mark on any metal surface with a graphite pencil or any type of sharp, pointed instrument. Temporary markings (defined as markings soluble in water or methyl chloro­ form) should be used for metal layout work or marking on the aircraft to indicate corroded ar­ eas.

d. Graphite should not be used as a lu­ bricant for any component. Graphite is ca­ thodic to all structural metals and will generate galvanic corrosion in the presence of moisture, especially if the graphite is applied in dry form.

e. Footwear and clothing should be in­ spected for metal chips, slivers, rivet cuttings, dirt, sand, etc., and all such material removed before walking or working on metal surfaces such as wings, stabilizers, fuel tanks, etc.

f. Do not abrade or scratch any surface unless it is an authorized procedure. If sur­ faces are accidentally scratched, the damage should be assessed and action taken to remove the scratch and treat the area.

g. Coated metal surfaces should not be polished for aesthetic purposes. Buffing would remove the protective coating and a brightly polished surface is normally not as corrosion resistant as a non-polished surface unless it is protected by wax or paint.

Page 6-18 Par 6-90

Page 290Open in PDF

h. Protect surrounding areas when welding, grinding, or drilling, to prevent con­ tamination with residue from these operations.

In those areas where protective covering can­ not be used, remove the residue by cleaning.

i. Severely corroded screws, bolts, and washers should be replaced. When a protec­ tive coating, such as a cadmium plating on bolts, or screws, is damaged, immediately ap­ ply an appropriate protective finish to prevent additional corrosion damage.

6-92.  6-112. [RESERVED.] Par 6-91 Page 6-19 (and 6-20)

Page 291Open in PDF

SECTION 7. BASIC CORROSION REMOVAL TECHNIQUES

6-113. GENERAL. When active corrosion is found, a positive inspection and rework pro­ gram is necessary to prevent any further dete­ rioration. The following methods of assessing corrosion damage and procedures for rework of corroded areas could be used during cleanup programs. In general, any rework would in­ volve the cleaning and stripping of all finish from the corroded area, removal of corrosion products, and restoration of surface protective film.

a. Repair of corrosion damage includes removal of all corrosion and corrosion prod­ ucts. When the corrosion damage is severe and exceeds the damage limits set by the air­ craft or parts manufacturer, the part must be replaced.

b. If manufacturer information and limits are not available, then a DER must be consulted before the aircraft or part is returned to service.

6-114. PREPARATIONS FOR REWORK.

All corrosion products should be removed completely when corroded structures are re­ worked. Before starting rework of corroded areas, carry out the following:

a. Document corrosion damage.

b. Position the aircraft in a wash rack or provide washing apparatus for rapid rinsing of all surfaces.

c. Connect a static ground line from the aircraft to a grounding point.

d. Prepare the aircraft for safe ground maintenance.

(1) Remove battery(s), liquid oxygen generator container (if installed), and external hydraulic and electric power.

(2) Install all applicable safety pins, flags, and jury struts.

e. Protect the pitot-static ports, louvers, airscoops, engine opening, wheels, tires, mag­ nesium skin panels, and airplane interior from moisture and chemical brightening agents.

f. Protect the surfaces adjacent to rework areas from chemical paint strippers, corrosion removal agents, and surface treatment materi­ als.

6-115. FAIRING OR BLENDING RE - WORKED AREAS. All depressions result­ ing from corrosion rework should be faired or blended with the surrounding surface. Fairing can be accomplished as follows:

a. Remove rough edges and all corrosion from the damaged area. All dish-outs should be elliptically shaped with the major axis run­ ning spanwise on wings and horizontal stabi­ lizers, longitudinally on fuselages, and verti­ cally on vertical stabilizers. (Select the proper abrasive for fairing operations from table 6-1.)

b. In critical and highly stressed areas, all pits remaining after the removal of corro­ sion products should be blended out to prevent stress risers that may cause stress corrosion cracking. (See figure 6-14.) On a non-critical structure, it is not necessary to blend out pits remaining after removal of corrosion products by abrasive blasting, since this results in un­ necessary metal removal.

Par 6-113 Page 6-21

Page 292Open in PDF

TABLE 6-1. Abrasives for corrosion removal.

METALS OR

MATERIALS TO BE

PROCESSED

RESTRICTIONS OPERATION ABRASIVE PAPER OR CLOTH ABRASIVE

FABRIC OR PAD

ALUMINUM STAINLESS STEEL PUMICE 350

MESH OR FINER

ABRASIVE WHEEL

ALUMINUM OXIDE

SILICON

CARBIDE GARNET

FERROUS ALLOYS

CORROSION

REMOVAL

OR FAIRING 150 GRIT

OR FINER 180 GRIT

OR FINER

FINE TO

ULTRA FINE

X X X X FINISHING 400 X X X

ALUMINUM AL- LOYS

EXCEPT CLAD

ALUMINUM

DO NOT USE

SILICON

CARBIDE

ABRASIVE

CORROSION

REMOVAL

OR FAIRING 150 GRIT

OR FINER 7/0 GRIT

OR FINER

VERY FINE AND

ULTRA FINE X X X FINISHING 400 X X CLAD

ALUMINUM

SANDING

LIMITED TO THE

REMOVAL OF MINOR

SCRATCHES

CORROSION

REMOVAL

OR FAIRING 240 GRIT

OR FINER 7/0 GRIT

OR FINER

VERY FINE AND

ULTRA FINE X X FINISHING 400 X

MAGNESIUM ALLOYS

CORROSION

REMOVAL

OR FAIRING 240 GRIT

OR FINER

VERY FINE AND

ULTRA FINE X X X FINISHING 400 X X

TITANIUM CLEANING AND

FINISHING 150 GRIT

OR FINER 180 GRIT

OR FINER X X X

c. Rework depressions by forming smoothly blended dish-outs, using a ratio of 20:1, length to depth. (See figure 6-15.) In areas having closely spaced multiple pits, in­ tervening material should be removed to minimize surface irregularity or waviness.

(See figure 6-16.) Steel nut-plates and steel fasteners should be removed before blending corrosion out of aluminum structure. Steel or copper particles embedded in aluminum can become a point of future corrosion. All corro­ sion products must be removed during blend­ ing to prevent reoccurrence of corrosion.

6-116. CORROSION REMOV AL BY BLASTING . Abrasive blasting is a process for cleaning or finishing ferrous metals by di­ recting a stream of abrasive particles against the surface of the parts. Abrasive blasting is used for the removal of rust and corrosion and for cleaning prior to painting or plating. The following standard blast-cleaning practices should be adopted.

a. The part to be blast-cleaned should be removed from the aircraft, if possible. Other­ wise, areas adjacent to the part should be masked or protected from abrasive impinge­ ment and system (hydraulic, oil, fuel, etc.)

contamination.

b. Parts should be dry and clean of oil, grease, or dirt, prior to blast cleaning.

c. Close-tolerance surfaces, such as bushings and bearing shafts, should be masked.

d. Blast-clean only enough to remove cor­ rosion coating. Proceed immediately with sur­ face treatments as required.

6-117. CLEANERS, POLISHES, AND BRIGHTENERS. It is important that aircraft be kept thoroughly clean of contaminating de­ posits such as oil, grease, dirt, and other for­ eign materials.

Page 6-22 Par 6-115

Page 293Open in PDF

FIGURE 6-14. Typical example of acceptable cleanup of corrosion pits.

a. Materials. Do not use harmful clean­ ing, polishing, brightening, or paint-removing materials. Use only those compounds that conform to existing government or established industry specifications or that have been spe­ cifically recommended by the aircraft manu­ facturer. Observe the product manufacturer’s recommendations concerning use.

b. Chemical Cleaners. Chemicals must be used with great care in cleaning assembled aircraft. The danger of entrapping corrosive materials in faying surfaces and crevices counteracts any advantages in their speed and effectiveness. Use materials that are relatively neutral and easy to remove.

c. Removal of spilled battery acid. The battery, battery cover, battery box and adjacent areas will be corroded if battery acid spills onto them. To clean spilled battery acid, brush off any salt residue and sponge the area with fresh water. For lead-acid batteries, sponge the area with a solution of 6 ounces of sodium bicarbonate (baking soda) per gallon of fresh water. Apply generously until bubbling stops and let solution stay on the area for 5 to 6 minutes, but do not allow it to dry. For nickel-cadmium batteries, sponge the area with a solution of 6 ounces of monobasic sodium phosphate per gallon of fresh water. Sponge area again with clean fresh water and dry sur­ face with compressed air or clean wiping cloths.

6-118. STANDARD METHODS. Several standard mechanical and chemical methods are available for corrosion removal. Mechanical methods include hand sanding using abrasive mat, abrasive paper, or metal wool; and pow­ ered mechanical sanding, grinding, and buff­ ing, using abrasive mat, grinding wheels, sanding discs, and abrasive rubber mats. The method used depends upon the metal and de­ gree of corrosion. The removal method to use on each metal for each particular degree of corrosion is outlined in the following section.

Par 6-117 Page 6-23

Page 294OCROpen in PDF

PIT HAS BEEN CLEANED UP TO THE EXTENT THAT

ALL LOOSE CORROSION PRODUCTS HAVE BEEN REMOVED.

CORROSION DAMAGE BEFORE REWORK

LONGITUDINAL

ROUGH EDGES HAVE BEEN SMOOTHED AND ALL CORROSION HAS BEEN REMOVED. HOWEVER, DEPRESSION HAS NOT BEEN SHAPED. DISH-OUT AFTER BLENDING FIGURE 6-15. Blendout of corrosion as a single depression.

CORROSION DAMAGE MIN- _10D - TRANSVERSE

BEFORE REMOVAL Ç5D - LONGITUDINAL MIN

BOTTOM OF DEPRESSION

AFTER CORROSION REMOVAL

AMAGE REMOVED AND SURFACE SMOOTHE

VITH SHALLOW ELLIPTICAL DISH-OU FIGURE 6-16. Blendout of multiple pits in a corroded area.

6-119.-6-131. [RESERVED.] Page 6-24 Par 6-118

Page 295Open in PDF

SECTION 8. ALUMINUM AND ALUMINUM ALLOYS

6-132. GENERAL. Aluminum and alumi­ num alloys are the most widely used material for aircraft construction. Aluminum appears high in the electro-chemical series of elements and corrodes very easily. However, the forma­ tion of a tightly-adhering oxide film offers in­ creased resistance under most corrosive condi­ tions. Most metals in contact with aluminum form couples that undergo galvanic corrosion attack. The alloys of aluminum are subject to pitting, intergranular corrosion and intergranular stress corrosion cracking. In some cases the corrosion products of metal in con­ tact with aluminum are corrosive to aluminum.

Therefore, aluminum and its alloys must be cleaned and protected.

6-133. SPECIAL TREATMENT OF ANODIZED SURFACES. Anodizing is the most common surface treatment of aluminum alloy surfaces. The aluminum sheet or casting is made the positive pole in an electrolyte bath in which chromic acid or other oxidizing agents produce a supplemental protective ox­ ide film on the aluminum surface. The ano­ dized surface coating offers the alloy a great deal of protection as long as it is not damaged.

Once the film is damaged, it can only be par­ tially restored by chemical surface treatment.

Therefore exercise care to avoid breaking of the protective film, particularly at the edges of the sheet.

6-134. REPAIR OF ALUMINUM ALLOY SHEET METAL. After extensive corrosion removal the following procedures should be followed:

a. If water can be trapped in blended ar­ eas, chemical conversion coat in accordance with MIL-C-81706 and fill the blended area with structural adhesive or sealant to the same level and contour as the original skin. When areas are small enough that structural strength has not been significantly decreased, no other work is required prior to applying the protec­ tive finish.

b. When corrosion removal exceeds the limits of the structural repair manual, contact a DER or the aircraft manufacturer for repair in­ structions.

c. Where exterior doublers are installed, it is necessary to seal and insulate them ade­ quately to prevent further corrosion.

d. Doublers should be made from alclad, when available, and the sheet should be ano­ dized (preferred) or a chemical conversion coat applied after all cutting, drilling, and counter­ sinking has been accomplished.

e. All rivet holes should be drilled, coun­ tersunk, surface treated, and primed prior to installation of the doubler.

f. Apply a suitable sealing compound in the area to be covered by the doubler. Apply sufficient thickness of sealing compound to fill all voids in the area being repaired.

g. Install rivets wet with sealant. Suffi­ cient sealant should be squeezed out into holes so that all fasteners, as well as all edges of the repair plate, will be sealed against moisture.

h. Remove all excess sealant after fasten­ ers are installed. Apply a fillet sealant bead around the edge of the repair. After the sealant has cured apply the protective paint finish to the reworked area.

Par 6-132 Page 6-25

Page 296Open in PDF

6-135. CORROSION REMOV AL

AROUND COUNTERSUNK FASTENERS IN ALUMINUM ALLOY. Intergranular cor­ rosion in aluminum alloys often originates at countersunk areas where steel fasteners are used.

a. When corrosion is found around a fixed fastener head, the fastener must be re­ moved to ensure corrosion removal. All cor­ rosion must be removed to prevent further cor­ rosion and loss of structural strength. To re­ duce the recurrence of corrosion, the panel should receive a chemical conversion coating, be primed, and have the fasteners installed wet with sealant.

b. Each time removable steel fasteners are removed from access panels, they should be inspected for condition of the plating. If mechanical or plating damage is evident, re­ place the fastener. One of the following fas­ tener installation methods should be used:

(1) Brush a corrosion-preventive com­ pound on the substructure around and in the fastener hole, start the fastener, apply a bead of sealant to the fastener countersink, set and torque the fastener within the working time of the sealant (this is the preferred method).

(2) Apply the corrosion preventive compound to the substructure and fastener, set and torque the fastener.

(3) Apply a coating of primer to the fastener, and while wet with primer, set and torque the fastener.

6-136. EXAMPLES OF REMOVING

CORROSION FROM ALUMINUM AND ALUMINUM ALLOYS.

a. Positively identify the metal as alumi­ num.

b. Clean the area to be reworked. Strip paint if required.

c. Determine extent of corrosion damage.

d. Remove light to moderate corrosion with one of the following.

(1) Non-Powered Corrosion Removal.

(a) The removal of corrosion prod­ ucts by hand can be accomplished by use of aluminum grit and silicon carbide abrasive, such as non-woven, non-metallic, abrasive mat (Spec. MIL-A-9962), abrasive cloth, and pa­ per. Aluminum wool, fiber bristle brushes, and pumice powder are also acceptable methods.

(b) Stainless steel brush (Spec.

H-B-178, type III, class 2) may be used as long as the bristles do not exceed 0.010 inch in di­ ameter. After use of this brush the surface should be polished with 60 grit aluminum ox­ ide abrasive paper, then with 400 grit alumi­ num oxide paper. Care should be exercised in any cleaning process to avoid breaking the protective film.

(c) Steel wool, emery cloth, steel wire brushes (except stainless steel brush) copper alloy brushes, rotary wire brushes, or severe abrasive materials should not be used on any aluminum surface.

(2) Chemical Corrosion Removal.

(a) The corrosion removal compound aluminum pretreatment MIL-C-38334, an acid material, may be used to remove corrosion products from aluminum alloy materials or items (e.g., skins, stringer, ribs in wings, tub­ ing, or ducts). MIL-C-38334 is available in two types:

1 Type I Liquid concentrate mate­ rials should be diluted in accordance with the Page 6-26 Par 6-135

Page 297Open in PDF

manufacture’s instructions before use. Type I has a 1 year shelf life; therefore it shall not be used after 1 year from the date of manufacture.

2 Type II Powdered concentrate materials should be dissolved in the volume of water specified on the kit. These materials have an indefinite shelf life in the dry state.

Once mixed, they should be used within 90 days.

(b) Mix MIL-C-38334 in wood, plastic, or plastic-lined containers only. Wear acid-resistant gloves, protective mask and protective clothing when working with this acid compound. If acid contacts the skin or eyes, flush immediately with water.

(c) Apply MIL-C-38334 solution by flowing, mopping, sponging, brushing, or wiping. When applying the solution to large areas, begin the application at the lowest area and work upward, applying the solution with a circular motion to disturb the surface film and ensure proper coverage. If pumping is re­ quired, pumps, valves, and fittings should be manufactured from 18-8 stainless steel or plastic.

CAUTION: When working with MIL-C-38334, keep the solution away from magnesium surfaces. The solu - tion must be confined to the area be - ing treated. All parts and assemblies including cadmium-plated items and hinges susceptible to damage from acid should be masked and/or protected. Also mask all openings leading to the primary structure that could trap the solution and doors or other openings that would allow the solution (uncontrolled) to get into the aircraft or equipment interior. It is a good practice to keep a wet rag on hand at all times, for removal of spills or splashes.

(d) Allow the solution to remain on the surface for approximately 12 minutes and then rinse away with clean tap water. For pit­ ted or heavily-corroded areas the compound will be more effective if applied warm (140 °F) followed by vigorous agitation with a non-metallic acid-resisting brush or aluminum oxide abrasive nylon mat. Allow sufficient dwell time, 12 to 15 minutes, before rinsing.

After each application examine the pits and/or corroded area to determine if another applica­ tion is required with a 4 to 10 power magnify­ ing glass. (Select the power depending on the distance available to make the inspection.)

Corrosion still on the area will appear as a powdery crust slightly different in color than the uncorroded base metal. Darkening of area due to shadows and reaction from the acid re­ mover should not be considered.

(e) Once the corrosion has been re­ moved and the area well-rinsed with clean water, a chromate conversion coating such as MIL-C-81706 or MIL -C-5541 alodine 1200, must be applied immediately thereafter.

e. Remove moderate to heavy corrosion with one of the following.

(1) Powered Corrosion Removal.

(a) Where the problem is severe enough to warrant the use of power tools, a pneumatic drill motor driving either an alumi­ num-oxide-impregnated nylon abrasive wheel, flap brush or rubber grinding wheel may be used with an abrasive value to approximately 120 grit, as needed. Corrosion-removal acces­ sories, such as flap brushes or rotary files, should be used on one type of metal only. For example, a flap brush used to remove alumi­ num should not be used to remove magnesium, steel, etc. Pneumatic sanders may be used with disk and paper acceptable for use on alu­ minum.

Par 6-136 Page 6-27

Page 298Open in PDF

(b) When mechanically removing corrosion from aluminum, especially aircraft skin thinner than 0.0625 inch, extreme care must be used. Vigorous, heavy, continuous abrasive grinding can generate enough heat to cause metallurgical change. If heat damage is suspected, hardness tests or conductivity tests must be accomplished to verify condition of the metal. The use of powered rotary files should be limited to heavy corrosion and should not be used on skin thinner than

0.0625 inch.

(2) Blasting.

(a) Abrasive blasting may be used on aluminum alloys using glass beads (Spec.

MIL-G-9954) sizes 10 to 13, or grain abrasive (Spec. MIL -G-5634) types I and III may be used as an alternate method of removing cor­ rosion from clad and non-clad aluminum al­ loys. Abrasive blasting should not be used to remove heavy corrosion products. Direct pres­ sure machines should have the nozzle pressure set at 30 to 40 psi for clad aluminum alloys and 40 to 45 psi for non-clad aluminum alloys.

Engineering approval should be obtained prior to abrasive blasting metal thinner than

0.0625 inch.

(b) When using abrasive blasting on aluminum alloys, do not allow the blast stream to dwell on the same spot longer than 15 seconds. Longer dwell times will cause ex­ cessive metal removal. Intergranular exfolia­ tion corrosion is not to be removed by abrasive blasting; however, blasting may be used with powered corrosion removal to determine whether all exfoliation corrosion has been re­ moved.

f. Inspect the area for remaining corro­ sion. Repeat procedure if any corrosion re­ mains.

NOTE: If corrosion remains after the second attempt, use a stronger method, e.g., chemical to mechanical.

g. Using a blend ratio of 20:1 (length to depth) blend and finish the corrosion rework area with progressively finer abrasive paper until 400-grit paper is used.

h. Clean reworked area using dry cleaning solvent. Do not use kerosene or any other pe­ troleum base fuel as a cleaning solvent.

i. Determine depth of faired depressions to ensure that rework limits have not been ex­ ceeded.

j. Apply chemical conversion coating, MIL-C-81706, immediately after reworking. If 48 hours or more have elapsed since the con­ version coating was first applied and the primer or final paint system has not yet been applied, then reapply the conversion coating before continuing.

NOTE: These solutions should not be allowed to come in contact with magnesium or high-strength steels (180,000 psi). Do not permit solutions or materials to contact paint thinner, acetone or other combustible material:

FIRE MAY RESULT.

k. Apply paint finish to area.

6-137.  6-147. [RESERVED.] Page 6-28 Par 6-136

Page 299Open in PDF

SECTION 9. MAGNESIUM AND MAGNESIUM ALLOYS

6-148. GENERAL. Magnesium and mag­ nesium alloys are the most chemically active of the metals used in aircraft construction and are the most difficult to protect. However, cor­ rosion on magnesium surfaces is probably the easiest to detect in its early stages. Since mag­ nesium corrosion products occupy several times the volume of the original magnesium metal destroyed, initial signs show a lifting of the paint films and white spots on the magne­ sium surface. These rapidly develop into snow-like mounds or even white whiskers.

The prompt and complete correction of the coating failure is imperative if serious struc­ tural damage is to be avoided.

6-149. TREATMENT OF WROUGHT MAGNESIUM SHEETS AND FORGINGS.

Corrosive attack on magnesium skins will usu­ ally occur around the edges of skin panels, un­ derneath hold-down washers, or in areas physically damaged by shearing, drilling, abra­ sion, or impact. Entrapment of moisture under and behind skin crevices is frequently a con­ tributing factor. If the skin section can be eas­ ily removed, this should be accomplished to ensure complete inhibition and treatment.

a. Complete mechanical removal of cor­ rosion products should be practiced when practical. Mechanical cleaning should nor­ mally be limited to the use of stiff bristle brushes and similar nonmetallic cleaning tools.

b. Any entrapment of steel particles from steel wire brushes, steel tools, or con­ tamination of treated surfaces, or dirty abra­ sives, can cause more trouble than the initial corrosive attack. The following procedural summary is recommended for treatment of cor­ roded magnesium areas when accomplished under most field conditions.

c. When aluminum insulating washers are used and they no longer fasten tightly to magnesium panels, corrosion is likely to occur under the washers if corrective measures are not taken.

(1) When machine screw fasteners are used, aluminum insulating washers must be removed from all locations to surface treat the magnesium panel.

(2) Where permanent fasteners other than machine screws are used, the insulating washer and fastener must be removed.

(3) When located so water can be trapped in the counter-bored area where the washer was located, use sealants to fill the counterbore. If necessary, fill several areas adjacent to each other. It may be advantageous to cover the entire row of fasteners with a strip of sealant.

6-150. REPAIR OF MAGNESIUM

SHEET METAL AFTER EXTENSIVE CORROSION REMOV AL. The same gen­ eral instructions apply when making repairs in magnesium as in aluminum alloy skin, except that two coats of epoxy primer may be re­ quired on both the doubler and skin being patched instead of one. Where it is difficult to form magnesium alloys in the contour, alumi­ num alloy may be utilized. When this is done, it is necessary to ensure effective dissimilar metal insulation. Vinyl tape will ensure posi­ tive separation of dissimilar metals, but edges will still have to be sealed to prevent entrance of moisture between mating surfaces at all points where repairs are made. It is recom­ mended that only non-corrosive type sealant be used, since it serves a dual purpose of material separation and sealing.

Par 6-148 Page 6-29

Page 300Open in PDF

6-151. IN-PLACE TREATMENT OF MAGNESIUM CASTINGS . Magnesium castings, in general, are more porous and more prone to penetrating attack than wrought mag­ nesium skin. However, treatment in the field is, for all practical purposes, the same for all magnesium. Bellcranks, fittings, and numer­ ous covers, plates, and handles may also be magnesium castings. When attack occurs on a casting, the earliest practical treatment is re­ quired to prevent dangerous corrosive penetra­ tion. Engine cases in salt water can develop moth holes and complete penetration over­ night.

a. If at all practical , faying surfaces in­ volved shall be separated to treat the existing attack effectively and prevent its further prog­ ress. The same general treatment sequence as detailed for magnesium skin should be fol­ lowed. Where engine cases are concerned, baked enamel overcoats are usually involved rather than other top coat finishes. A good air drying enamel can be used to restore protec­ tion.

b. If extensive removal of corrosion products from a structural casting is involved, a decision from the aircraft manufacturer or a DER may be necessary to evaluate the ade­ quacy of structural strength remaining. Refer to the aircraft manufacturer if any questions of safety are involved.

6-152. EXAMPLE OF REMOVING CORROSION FROM MAGNESIUM . If possible, corroded magnesium parts shall be removed from aircraft. When impossible to remove the part, the following procedure will be used.

a. Positively identify metal as magnesium.

b. Clean area to be reworked.

c. Strip paint if required.

d. Determine the extent of corrosion damage.

e. Remove light to moderate corrosion by one of the following means.

(1) Non-Powered Corrosion Removal.

(a) Non-powered removal can be ac­ complished using abrasive mats, cloth, and pa­ per with aluminum oxide grit (do not use sili­ con carbide abrasive). Metallic wools and hand brushes compatible with magnesium such as stainless steel and aluminum, may be used.

(b) When a brush is used the bristles should not exceed 0.010 inch in diameter.

After using a brush, the surface should be pol­ ished with 400 grit aluminum oxide abrasive paper, then with 600 grit aluminum oxide abrasive paper.

(c) Pumice powder may be used to remove stains or to remove corrosion on thin metal surfaces where minimum metal removal is allowed.

(2) Chemical Corrosion Removal.

(a) Chemical corrosion removal on magnesium alloys is usually done with a chromic acid pickle solution. Chemical corro­ sion removal methods are not considered ade­ quate for areas that have:

1 Deep pitting, 2 Heavy corrosion and corrosion by products, 3 Previously had corrosion re­ moved by mechanical means, or 4 Previously been sand blasted.

Page 6-30 Par 6-151