(b) Do not use this method for parts containing copper and steel-based inserts (un less the inserts are masked off) and where it might come into contact with adhesive bonded skins or parts.
(3) The following solution may be used to remove surface oxidation and light corro sion products from magnesium surfaces.
(a) Solution Composition and Op eration:
1 Chromium Trioxide. 24 oz.
2 (O-C-303, Type II). Water to Make 1 gal. Reaction Time 1 to 15 min.
3 Operation Temperature. (Solu tion can be operated at room temperature for a longer reaction time if desired.) 190 to 202 °F.
4 Container Construction. Leadlined steel, stainless steel, or 1100 aluminum.
(b) Mask off nearby operating mechanisms, cracks and plated steel to keep the solution from attacking them.
(c) Apply chromic acid solution care fully to the corroded area with an acid-resistant brush.
(d) Allow the solution to remain on the surface for approximately 15 minutes.
Agitation may be required.
(e) Thoroughly rinse the solution from the surface with plenty of clean water.
(f) Repeat the preceding sequence as necessary until all corrosion products have been removed and the metal is a bright metal lic color.
f. Remove moderate to heavy corrosion by one of the following means.
(1) Powered Corrosion Removal.
(a) Powered corrosion removal can be accomplished using pneumatic drill motor with either an aluminum-oxide-impregnated abrasive wheel, flap brush, or rubber grinding wheel with an abrasive value to approximately 120 grain size.
(b) Also a rotary file with fine flutes can be used for severe or heavy corrosion product buildup on metals thicker than
0.0625 inch. If a flap brush or rotary file is used, it should only be used on one type of metal. Do not use either a hand or rotary car bon steel brush on magnesium.
(c) Pneumatic sanders are acceptable if used with disk or paper of aluminum oxide.
When using sanders, use extra care to avoid over heating aircraft skins thinner than
0.0625 inch.
(d) Do not use rotary wire brushes on magnesium.
WARNING: Cuttings and small shavings from magnesium can ignite easily and are an extreme fire hazard.
Fires of this metal must be extin - guished with absolutely dry talc, calcium carbonate, sand, or graphite by applying the powder to a depth of 1/2 inch over the metal.
(2) Blasting. Abrasive blasting is an approved method of corrosion removal on magnesium alloys of a thickness greater than
0.0625 inch. Remove heavy corrosion prod ucts by hand brushing with a stainless steel or fiber brush followed by vacuum abrasive Par 6-152 Page 6-31
blasting with glass beads, (Spec. MIL-G-9954) sizes 10-13; or grain abrasive (Spec.
MIL-G-5634), types I or III at an air pressure of 10 to 35 psi (if suction equipment is used, use a 50 percent higher pressure). Upon com pletion of blasting, inspect for the presence of corrosion in the blast area. Give particular at tention to areas where pitting has progressed into intergranular attack. This is necessary be cause abrasive blasting has a tendency to close up streaks of intergranular corrosion rather than remove them if the operator uses an im proper impingement angle. If the corrosion has not been removed in a total blasting time of 60 seconds on any one specific area, other mechanical methods of removal should be utilized.
CAUTION: When blasting magnesium alloys, do not allow the blast stream to dwell on the same spot longer than 15 seconds. Longer dwell times will cause excessive metal re - moval.
g. Inspect the reworked area to ensure that no corrosion products remain. If corrosion products are found, repeat method used and re-inspect.
h. Fair depressions resulting from rework using a blend ratio of 20:1. Clean rework area using 240 grit abrasive paper. Smooth with 300 grit and finally polish with 400 grit abra sive paper.
i. Determine depth of faired depressions to ensure that rework limits have not been ex ceeded. Refer to the manufacture’s specifica tions.
j. Clean reworked area using a solvent to provide a water-break-free surface. Do not use kerosene or another petroleum base fuel as a cleaning solvent.
k. Apply Chromic Acid Brush-on Pre treatment.
(1) Chemical pretreatment such as the following chromic acid solution (Conversion coat conforming to Spec. MIL-M-3171, type VI) provides a passive surface layer with an inhibitive characteristic that resists corro sive attack and also provides a bond for subse quent coatings. Properly-applied magnesium pretreatment tend to neutralize corrosion me dia in contact with the surface.
(2) The chromic acid brush-on pre treatment may be applied to all magnesium parts that require touch-up. This treatment is generally used in refinishing procedures or when parts and assemblies are too large to be immersed. This treatment is less critical to ap ply than the other brush-on treatments. It is relatively inexpensive and not as harmful when trapped in faying surfaces.
(a) Solution Composition and Op eration:
1 Distilled Water 1 gal.
2 Chromic Acid (CrO3) 1.3 oz.
3 (99.5 pure), Calcium Sulfate 1 oz. (CaSo4.2H2O) 4 Operating Temp. 70-90 °F.
5 Container: Stainless Steel, Alu minum, Vinyl, Polyethylene, or Rubber.
NOTE: Good application requires proper preparation of the chromic acid coating solution and cleaning of the surface where the solution will be applied. A water-break test is recom - mended if the cleanliness of the surface is in doubt.
Page 6-32 Par 6-152
(b) Add chemicals to water in the or der shown.
(c) Stir vigorously for at least 15 minutes, either mechanically or by air agi tation, to ensure that the solution is saturated with calcium sulfate. (Let solution stand for 15 minutes before decanting.)
(d) Prior to use, decant solution (avoid transfer of undissolved calcium sulfate) into suitable containers (polyethylene or glass).
(e) Apply solution by brush, swab, or flow on using low-pressure spray (non atomizing) until the metal surface becomes a dull color (the color can vary from greenbrown, brassy, yellow-brown to dark-brown).
For good paint adhesion, a dark-brown color free of powder is considered best. The color may vary in using different vendors’ materials.
NOTE: Too long an exposure to the brush-on solution produces coatings that will powder and impair adhesion of applied paint finish/films.
(f) Observe the coating closely dur ing the treatment for color changes, rinsed with cold running water when the desired condi tion/color is reached and air dried. Preparation and use of test panels made of the same mate rial and under the same conditions, before starting the actual treating operation may be used as to determine the application time re quired to produce the required coating. A good coating is uniform in color/density, ad heres well and is free of loose powder.
l. Apply primer and top coat finish
m. Remove masking and protective cov erings.
6-153. 6-163. [RESERVED.] Par 6-152 Page 6-33 (and 6-34)
SECTION 10. FERROUS METALS
6-164. GENERAL. One of the most famil iar kinds of corrosion is red iron rust. Red iron rust results from atmospheric oxidation of steel surfaces. Some metal oxides protect the un derlying base metal, but red rust is not a pro tective coating. Its presence actually promotes additional attack by attracting moisture from the air and acts as a catalyst to promote addi tional corrosion.
a. Red rust first shows on bolt heads, hold down nuts, and other unprotected aircraft hardware. Red rust will often occur under nameplates that are secured to steel parts. Its presence in these areas is generally not dan gerous. It has no immediate effect on the structural strength of any major components.
However, it shows a general lack of mainte nance and may indicate attack in more critical areas.
b. When paint failures occur or me chanical damage exposes highly-stressed steel surfaces to the atmosphere, even the smallest amount of rusting is potentially dangerous and should be removed immediately.
6-165. SPECIAL TREATMENT OF HIGH-STRENGTH STEEL. (High-strength steels heat treated above Rockwell C40, 180,000 psi tensile strength). Any corrosion on the surface of a highly-stressed steel part is potentially dangerous, and the careful removal of corrosion products is mandatory. Surface scratches or change in surface structure from overheating can cause sudden failure of these parts. The removal of corrosion products is required and will be performed carefully and completely.
a. Acceptable methods include careful use of mild abrasive mats, cloths, and papers, such as fine grit aluminum oxide, metallic wool, or fine buffing compounds.
b. Undesirable methods include the use of any power tool because the danger of local overheating and the formation of notches that could lead to failure. The use of chemical cor rosion removers is prohibited, without engi neering authorization, because high-strength steel parts are subject to hydrogen embrittle ment.
6-166. SPECIAL TREATMENT OF STAINLESS STEEL. Stainless steels are of two general types: magnetic and nonmagnetic.
a. Magnetic steels are of the ferritic or martensitic types and are identified by num bers in the 400-series. Corrosion often occurs on 400-series stainless steels and treatment is the same as specified in high-strength steels.
(See paragraph 6-165.)
b. Non-magnetic stainless steels are of the austenitic type and are identified by num bers in the 300-series. They are much more corrosion resistant than the 400-series steels, particularly in a marine environment.
(1) Austenitic steels develop corrosion resistance by an oxide film, which should not be removed even though the surface is discol ored. The original oxide film is normally formed at time of fabrication by passivation. If this film is broken accidentally or by abrasion, it may not restore itself without repassivation.
(2) If any deterioration or corrosion does occur on austenitic steels, and the struc tural integrity or serviceability of the part is af fected, it will be necessary to remove the part.
Par 6-164 Page 6-35
6-167. EXAMPLE OF REMOVING
CORROSION FROM FERROUS MET - ALS. If possible, corroded steel parts should be removed from the aircraft. When impracti cal to remove the part, follow the procedure below.
a. Prepare the area for rework.
b. Positively identify the metal as steel and establish its heat-treated value.
c. Clean the area and strip paint if re quired.
NOTE: Use of acid-based strippers, chemical removers, or chemical con - version coatings are not permitted on steel parts without engineering authorization.
d. Determine extent of corrosion damage.
e. Remove residual corrosion by hand sanding with mild abrasive mats, cloths, and papers, such as fine aluminum oxide grit.
f. Remove heavy deposits of corrosion products by approved mechanical methods for that particular form of steel and/or stainless steel.
g. Inspect the area for remaining corro sion. Repeat procedure if any corrosion re mains and the structural integrity of the part is not in danger, and the part meets the rework limits established by the manufacturer or FAA authorized DER.
h. Fair depressions using a blend ratio of 20:1. Clean area using 240-grit paper.
Smooth area with 300-grit paper and give final polish with 400-grit paper.
i. Determine depth of faired depression to ensure that rework limits have not been ex ceeded.
j. Clean reworked area with dry cleaning solvent. Do not use kerosene.
k. Apply protective finish or specific or ganic finish as required.
NOTE: Steel surfaces are highlyreactive immediately following corrosion removal; consequently, primer coats should be applied within 1 hour after sanding.
l. Remove masking and protective cover ings.
6-168. 6-178. [RESERVED.] Page 6-36 Par 6-167
SECTION 11. OTHER METALS AND ALLOYS
6-179. NOBLE METAL COATINGS - CLEANUP AND RESTORATION . Silver, platinum, and gold finishes are used in aircraft assemblies because of their resistance to ordi nary surface attack and their improved electri cal or heat conductivity. Silver-plated elec trodes can be cleaned of brown or black sulfide tarnish, by placing them in contact with a piece of magnesium sheet stock while immersed in a warm water solution of common table salt mixed with baking soda or by using a fine grade abrasive mat or pencil eraser followed by solvent cleaning. If assemblies are in volved, careful drying and complete displace ment of water is necessary. In general, clean ing of gold or platinum coatings is not recom mended in the field.
6-180. COPPER AND COPPER ALLOYS are relatively corrosion resistant, and attack on such components will usually be limited to staining and tarnish. Such change in surface condition is not dangerous and should ordinar ily have no effect on the function of the part.
However, if it is necessary to remove such staining, a chromic acid solution of 8 to 24 ounces per gallon of water containing a small amount of battery electrolyte (not to exceed 50 drops per gallon) is an effective brightening bath. Staining may also be removed using a fine grade abrasive mat or pencil eraser fol lowed by solvent cleaning.
a. Immerse the stained part in the cold solution. Surfaces can also be treated in place by applying the solution to the stained surface with a small brush.
b. Avoid any entrapment of the solution after treatment. Clean the part thoroughly following treatment with all residual solution removed.
c. Serious copper corrosion is evident by the accumulation of green-to-blue copper salts on the corroded part. Remove these products mechanically using a stiff bristle brush, brass wire brush, 400-grit abrasive paper or bead blast with glass beads, (specification MIL-G-9954, size 13). Air pressure when blasting should be 20 to 30 psi for direct pres sure machines. Do not bead blast braided cop per flexible lines. Reapply a surface coating over the reworked area. Chromic acid treat ment will tend to remove the residual corro sion products.
WARNING: Brushing, sanding, and abrasive blasting of copper and copper alloys can be dangerous due to the creation of toxic airborne particles.
Take necessary precautions to ensure safety.
6-181. TITANIUM AND TITANIUM AL - LOYS are highly corrosion resistant because an oxide film forms on their surfaces upon contact with air.
a. When titanium is heated, different oxides having different colors form on the sur face. A blue oxide coating will form at 700 to 800 °F; a purple oxide at 800 to 950 °F; and a gray or black oxide at 1000 °F or higher.
These coatings are protective discolorations and should not be removed.
b. Corrosive attack on titanium surfaces is difficult to detect. It may show deterioration from the presence of salt deposits and metal impurities at elevated temperatures so periodic removal of surface deposits is required. How ever, if corrosion develops on titanium, it usu ally occurs as pitting. Acceptable methods for corrosion removal are:
Par 6-179 Page 6-37
(1) Stainless steel wool or hand brush.
(2) Abrasive mats, cloths, and papers with either aluminum oxide or silicon carbide grit.
(3) Dry abrasive blasting using glass beads (spec. MIL-G-9954) sizes 10-13 or Aluminum oxide (spec. MIL-G-21380, type I, grades A or B) at a blast pressure of 40 to 50 psi (if using suction equipment use 50 percent higher pressure).
WARNING: Dry abrasive blasting of titanium alloys creates sparking. Ensure that hazardous concentrations of flammable vapors are not present.
(4) Hand polish with aluminum polish and soft cloth.
c. Titanium surfaces are susceptible to hydrogen embrittlement that can induce stress corrosion and associated pitting. Therefore, chemicals such as fire-resistant hydraulic flu ids must be controlled. Chlorinated hydrocar bon solvents and chemical corrosion removers are prohibited from use on titanium and tita nium alloys.
6-182. 6-192. [RESERVED.] Page 6-38 Par 6-181
SECTION 12. PLATED PARTS
6-193. CHROMIUM AND NICKEL - PLATED PARTS . Nickel and chromium platings are used extensively as protective and wear-resistant coatings over high-strength steel parts (landing gear journals, shock strut pis tons, etc.). Chromium and nickel plate provide protection by forming a somewhat impervious physical coat over the underlying base metal.
When breaks occur in the surface, the protec tion is destroyed.
a. The amount of reworking that can be performed on chromium and nickel-plated components is limited.
b. The rework should consist of light buffing to remove corrosion products and pro duce the required smoothness. The buffing should not take the plating below the mini mum allowable thickness.
c. Whenever a chromium or nickel-plated component requires buffing, coat the area with a corrosion-preventive compound, if possible.
d. When buffing exceeds the minimum thickness of the plating, or the base metal has sustained corrosive attack, the component should be removed and replaced.
e. The removed component can be re stored to serviceable condition by having the old plating completely stripped and replated in accordance with acceptable methods and specifications.
6-194. CADMIUM AND ZINC-PLATED PARTS. Cadmium plating is used extensively in aircraft construction as a protective finish over both steel and copper alloys. Protection is provided by a sacrificial process in which the cadmium is attacked rather than the un derlying base material. Properly functioning cadmium surface coatings may show mottling, ranging from white to brown to black spots on their surfaces. These show the sacrificial pro tection being offered by the cadmium coat, and under no condition should such spotting be removed merely for appearance sake. In fact, cadmium will continue to protect even when actual breaks in the coating develop and bare steel or exposed copper surfaces appear.
a. When the breakdown of the cad - mium plating occurs and the initial appear ance of corrosion products on the base metal develops, some mechanical cleaning of the area may be necessary but shall be limited to removal of the corrosion products from the underlying base material.
b. Under no condition should such a coating be cleaned with a wire brush. If pro tection is needed, a touch-up with primer or a temporary preservative coating should be ap plied. Restoration of the plate coating cannot be done in the field.
c. Zinc coatings offer protection in an identical manner to cadmium, and the correc tive treatment for failure is generally the same as for cadmium-plated parts. However, the amount of zinc on aircraft structures is very limited and usually does not present a mainte nance problem.
6-195. 6-205. [RESERVED.] Par 6-193 Page 6-39 (and 6-40)
SECTION 13. CORROSION PROOFING OF LAND PLANES
CONVERTED TO SEA PLANES
6-206. GENERAL. A special problem is encountered in the conversion of land planes to seaplanes. In general, land planes do not re ceive corrosion proofing to the same extent as do seaplanes. Corrosion-proofing standards for land planes converted to seaplanes are di vided into two classes, necessary minimum precautions and recommended precautions.
Regardless of such precautions, it is imperative that the exterior surfaces of seaplanes be washed with clear fresh water immediately following extended water operation, or at least once a day when operated in salty or brackish water. Wash interior surfaces of seaplanes ex posed to spray, taking care to prevent damage to electrical circuits or other items subject to injury.
6-207. NECESSARY MINIMUM PRE - CAUTIONS. The following procedures are considered the minimum to safeguard the air worthiness of converted aircraft and are not in themselves intended to maintain airworthiness for an indefinite period.
a. Unless already protected , treat ex posed fittings or fittings that can be reached through inspection openings with two coats of zinc chromate primer, paralketone, nonwater soluble heavy grease, or comparable materials.
This applies to items such as wing-root fit tings, wing-strut fittings, control-surface hinges, horns, mating edges of fittings, and at tached bolts.
b. Coat non-stainless control cables with grease or paralketone or other comparable protective coating, if not replaced with corro sion-resistant cables.
c. Inspect all accessible sections of air craft structure. Clean structural parts showing corrosion and refinish if corrosion attack is su perficial. If a part is severely corroded, replace with an adequately corrosion-proofed part.
6-208. RECOMMENDED PRECAUTIONS.
Recommended precautions are those which are suggested as a means of maintaining such air craft in condition for safe operation over ex tended periods.
a. Provide additional inspection openings to assist in detecting corrosion. Experience has shown openings to allow inspection of the lower and rearward portion of the fuselage to be particularly desirable.
b. Incorporate additional provisions for free drainage and ventilation of all interiors to prevent collection of moisture (scoop-type ma rine drain grommets).
c. Protect the interior of structural steel tubing. This may be done by air and watertight sealing or by flushing with hot linseed oil and plugging the openings. Inspect tubing for missing sealing screws, presence of entrapped water, local corrosion around sealing screws, welded clusters, and bolted fittings, which may be indicative of entrapped moisture.
d. Slit the fabric of fabric-covered aircraft longitudinally on the bottom of the fuselage and tail structure for access to these sections.
Coat the lower structural members with zinc chromate primer (two coats); follow by a coat of dope-proof paint or wrap with cellophane tape and rejoin the fabric. This precaution is advisable within a few months after start of operation as a seaplane.
e. Spray the interior of metal-covered wings and fuselages with an adherent corro sion inhibitor.
Par 6-206 Page 6-41
f. Place bags of potassium or sodium di chromate in the bottom of floats and boat hulls to inhibit corrosion.
g. Prevent the entry of water by sealing, as completely as possible, all openings in wings, fuselage, control-surface members, openings for control cables, tail-wheel wells, etc.
6-209. 6-219. [RESERVED.] Page 6-42 Par 6-208
SECTION 14. HANDLING AND CARE OF AIRCRAFT RECOVERED
FROM WATER IMMERSION.
6-220. GENERAL. Aircraft recovered from partial or total immersion in standing water or flash floods require an in-depth inspection and cleaning of both the exterior and interior areas.
Water-immersion increases the probability of corrosive attack, it removes lubricants, deterio rates aircraft materials, and destroys electrical and avionics components.
a. Sea water, because of salt content, is more corrosive than fresh water. However, fresh water may also contain varying amounts of salt and, as drying occurs, the salt concen tration is increased and corrosive attack accel erated.
b. Prompt action is the most important factor following recovery of an aircraft from water-immersion. Components of the aircraft which have been immersed, such as the powerplant, accessories, airframe sections, actuating mechanisms, screws, bearings, working surfaces, fuel and oil systems, wiring, radios, and radar should be disassembled, as necessary, and the contaminants completely removed.
6-221. INITIAL FRESH WATER OR DETERGENT WASH. As soon as possible after the aircraft is recovered from waterimmersion, thoroughly wash all internal and external areas of the aircraft using a wa ter/detergent solution as follows:
a. Mix liquid detergent (MIL-D-16791, type I) and isopropyl alcohol (TT-I-735) in ra tio of eight parts detergent, to 20 parts of alco hol. Add the detergent/alcohol mixture to 72 parts of tap water and mix thoroughly. For use, add one part of the preceding concentrate to nine parts of tap water (warm water if avail able) and mix thoroughly.
b. If the above specified deter gent/alcohol materials are not available, use water-emulsion cleaning compound (MIL-C-43616). Add one part compound to nine parts water. If the MIL cleaning com pound is not available, use any available mild household detergent solution with fresh tap water.
6-222. RECIPROCATING ENGINES AND PROPELLERS. Remove the propeller from the engine and the engine from the air craft. The exterior of the engine and propeller should be washed with steam, or fresh water, preferably hot.
a. Major accessories, engine parts, etc., should be removed and all surfaces flushed with fresh water, preferably hot. If facilities are available, immerse the removed parts, time permitting, in hot water or hot oil, 180 °F, for a short time. Soft water is preferred. Change the water frequently. All parts must be com pletely dried by air blast or other means. If no heat-drying facility is available, wipe the cleaned parts with suitable drying cloths.
b. The constant-speed propeller mecha nism should be disassembled, as required, to permit complete decontamination. Clean parts with steam or fresh water, preferably hot. Dry the cleaned parts in an oven, but if a heatdrying facility is not available, wipe the cleaned parts with suitable drying cloths.
6-223. AIRFRAME. The salvable compo nents of the fuselage, wings, empennage, sea plane and amphibian hulls and floats, and movable surfaces should be processed as fol lows:
Par 6-220 Page 6-43
a. The fabric from fabric-covered sur faces should be removed and replaced.
b. Clean the aircraft interior and exterior using steam under pressure with steam clean ing compound. Direct the steam into all seams and crevices where corrosive water may have penetrated. Avoid steam cleaning electrical equipment, such as terminal boards and re lays.
c. Areas that have been steam cleaned should be rinsed immediately with either hot or cold fresh water.
d. Touch up all scratches and scars on painted surfaces using zinc chromate primer or preservative.
e. Undrained hollow spaces or fluid en trapment areas should be provided temporary draining facilities by drilling out rivets at the lowest point. Install new rivets after drainage.
f. Remove and replace all leather, fabric upholstery, and insulation. Plastic or rubber foam that cannot be cleaned of all corrosive water must be replaced.
g. All drain plugs or drive screws in tu bular structures should be removed and the structure blown out with compressed air. If water has reached the tubular interiors, care fully flush with hot fresh water and blow out water with compressed air. Roll the structure as necessary to remove water from pockets.
Fill the tubes with hot linseed oil, approxi mately 180 °F, drain oil and replace drain plugs or drive screws.
h. Clean sealed wood, metallic, and other non-metallic areas, excluding acrylic plastics, with warm water. Replace wood, metalite, and other porous materials exposed to waterimmersion unless surfaces are adequately sealed to prevent penetration by water. Virtu ally all solvents and phenolic type cleaning agents are detrimental to acrylics and will ei ther soften the plastic or cause crazing.
i. Remove instruments and radios and ap plicable cables and plumbing, and repair and inspect as necessary.
6-224. 6-234. [RESERVED.] Page 6-44 Par 6-223